Preparation method of lithium ion battery negative electrode material based on hollow carbon nanocage
Through the preparation method of lithium-ion battery negative electrode material based on hollow carbon nanocage, the lack of energy and power density of lithium-ion battery negative electrode material in the prior art is solved, high capacity, rate performance and stability are achieved, and cost is reduced , meets the high-performance needs of power batteries.
Patent Information
- Application Number
- CN202411382357.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
The existing lithium-ion battery anode materials, especially graphite carbon materials, are difficult to meet the high energy density and power density required by power vehicles. At the same time, the nano-carbon cages have insufficient capacity and rate performance, which cannot effectively meet the higher lithium-ion battery. Energy and power density requirements.
Using the preparation method of lithium-ion battery negative electrode material based on hollow carbon nanocage, high-temperature sintering, acid treatment, grinding with binder, uniform coating and assembly of electrode sheets under inert gas, high-performance lithium Ion battery negative electrode material.
The high capacity performance, rate performance and stability of lithium-ion batteries are realized, and the cost is reduced. The charging and discharging voltage range is 0.05~3.0V, with high specific capacity and good cycle stability, and charge and discharge under different currents. The specific capacity did not drop at 1500 turns, and the energy density and power density reached a higher level.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and more particularly to a method for preparing a lithium ion battery negative electrode material based on hollow carbon nano cages. Background Art
[0002] With the successful application of lithium-ion batteries in low-power electronic devices, and under the dual pressure of fossil energy and environment, people have begun to explore the application of lithium-ion batteries in hybrid electric vehicles and pure electric vehicles. (Nature 2008, 451, 652; Chem. Rev. 2011, 111, 3577; Nano Lett. 2011, 11, 3785) However, the existing graphite carbon materials for the negative electrode of lithium-ion batteries are difficult to achieve the high energy density and power density required for power vehicles.
[0003] Therefore, the research on negative electrode materials used in power batteries has received extensive attention. Although a large number of studies on silicon-based and metal oxide negative electrode materials have been reported recently, they have poor cycle stability, rate performance and safety due to their large volume expansion during charge and discharge. (Nature 2001, 414, 3559; Science 2010, 330, 1515) Carbon materials have the advantages of high conductivity, stability, low price and environmental friendliness, so it is currently difficult to find a better negative electrode material than carbon materials. (Chem.Mater.2010,22,587) So far, many types of carbon nanomaterials have been studied as lithium-ion battery electrode materials, such as carbon nanotubes, (Electrochim.Acta 2005,51,23; Carbon 2002,40,1775) carbon nanofibers, (J.Phys.Chem.C2009,113,13438) carbon nanoonions (J.Phys.Chem.C2011,115,8923) and so on; especially graphene, which has been very popular recently, can achieve very high capacity density and power density, but still has poor stability and complex synthesis process. (Acs Nano 2011, 5, 3831; J. Am. Chem. Soc. 2010, 132, 12556; Carbon 2009, 47, 2049) In addition, related articles reported that the carbon nanocages synthesized by supercritical fluid method were used in the negative electrode materials of lithium-ion batteries, and the electrochemical performance was improved to a certain extent, but the material synthesis method was complicated. (J. Mater. Chem. 2010, 20, 9748; Chem. Mater. 2007, 19, 3349).
[0004] At present, the preparation of nano carbon cages is mainly based on the template method. CN101284663A discloses a method for preparing a large number of high-quality hollow carbon nano cages, which uses magnesium oxide as a template and prepares nano carbon cages by a vapor deposition method. The nano carbon cage has a large specific surface area and exhibits very excellent capacitance performance as a supercapacitor electrode. Hu et al. ("Carbon Nanocages as Supercapacitor Electrode Materials." Adv. Mater. 2012, 24, 347-352) prepared nano carbon cages using the template method, and its specific capacitance reached 260F / g.
[0005] The unique hollow structure and excellent conductivity of nanocarbon cages make them more widely used in the field of energy storage devices, and they are gradually becoming a potential substitute for graphite, the negative electrode material of lithium-ion batteries. However, nanocarbon cages also face the problems of low specific capacity and poor rate performance, and cannot meet the requirements of higher energy and power density of lithium-ion batteries. Summary of the invention
[0006] In view of this, the present invention provides a method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nanocages. The prepared negative electrode for a lithium ion battery has high capacity performance, rate performance, stability and lower cost.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A method for preparing a lithium ion battery negative electrode material based on hollow carbon nanocages comprises the following steps:
[0009] (1) sintering ammonium ferric citrate at high temperature under an inert gas, cooling, treating with acid, filtering, and drying to obtain carbon nanocages;
[0010] (2) dissolving the carbon nanocages and the binder in N-methylpyrrolidone and grinding them thoroughly in an agate mortar to obtain a black slurry;
[0011] (3) The black slurry is evenly coated on the current collector, and after drying, a carbon nanocage electrode plate is obtained, and the plate is punched for standby use;
[0012] (4) The electrode plates are placed in a glove box, and the electrolyte, metal lithium plates, gaskets, springs and button cell shells are used to assemble a lithium-ion battery.
[0013] Preferably, the high temperature sintering is sintering at 700-800° C. for 2-4 hours.
[0014] Preferably, the acid treatment is carried out in 1-2 mol / L hydrochloric acid at 50-80° C. for 15-20 h.
[0015] Preferably, the binder is PVDF.
[0016] Preferably, the mass ratio of the carbon nanocage to the binder is 5:1.
[0017] Preferably, the current collector is copper foil or aluminum foil.
[0018] Preferably, the drying is carried out in an electric hot air drying oven at 80° C. for 12 hours.
[0019] Preferably, the diameter of the carbon nanocage electrode plate is 10 mm.
[0020] Preferably, the atmosphere of the glove box has an oxygen content and a water content both less than 0.1 ppm.
[0021] Preferably, the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1.
[0022] It can be seen from the above technical solutions that, compared with the prior art, the present invention has the following technical effects:
[0023] The lithium ion battery obtained by the present invention has a charge and discharge voltage range of 0.05 to 3.0 V. -1 It has a high specific capacity of 1200mAh g -1 .
[0024] The lithium ion battery obtained by the invention has good stability, and the specific capacity does not decrease when it is charged and discharged for 1500 cycles at different currents (1.0, 10, 20, 25 A / g). DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] A method for preparing a lithium ion battery negative electrode material based on hollow carbon nanocages comprises the following steps:
[0028] (1) sintering ammonium ferric citrate under inert gas at 800° C. for 4 h, cooling and treating in 2 mol / L hydrochloric acid at 80° C. for 20 h, filtering and drying to obtain carbon nanocages;
[0029] (2) dissolving carbon nanocages and PVDF in N-methylpyrrolidone at a mass ratio of 5:1, and grinding them thoroughly in an agate mortar to obtain a black slurry;
[0030] (3) The black slurry is evenly coated on the current collector, dried in an electric hot air drying oven at 80° C. for 12 h, and cut into carbon nanocage electrode pieces with a diameter of 10 mm using a commercially available manual slicer, and the pieces are punched for later use;
[0031] (4) The electrode plates are placed in a glove box, and a lithium-ion battery is assembled using an electrolyte, a metal lithium plate, a gasket, a spring and a button battery shell; the atmosphere in the glove box has an oxygen content and a water content of less than 0.1 ppm; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1.
[0032] The lithium-ion battery obtained by this method has a first discharge capacity of 4500mAh g at a charge and discharge current density of 0.1A / g. -1 , reversible charge capacity is 1243 mAh g -1 After 30 cycles, the reversible specific capacity can still reach 823 mAh g -1 In terms of stability, the specific capacity did not decrease after 1500 cycles of charge and discharge at different currents (1.0, 10, 20, 25A / g). At a high current of 30A / g, it has a capacity of 210Wh kg electrode -1 Energy density is 69kWk gelectrode -1 High power density.
[0033] Example 2
[0034] A method for preparing a lithium ion battery negative electrode material based on hollow carbon nanocages comprises the following steps:
[0035] (1) sintering ammonium ferric citrate under inert gas at 700° C. for 2 h, cooling and treating in 1 mol / L hydrochloric acid at 50° C. for 15 h, filtering and drying to obtain carbon nanocages;
[0036] (2) dissolving carbon nanocages and PVDF in N-methylpyrrolidone at a mass ratio of 5:1, and grinding them thoroughly in an agate mortar to obtain a black slurry;
[0037] (3) The black slurry is evenly coated on the current collector, dried in an electric hot air drying oven at 80° C. for 12 h, and cut into carbon nanocage electrode pieces with a diameter of 10 mm using a commercially available manual slicer, and the pieces are punched for later use;
[0038] (4) The electrode plates are placed in a glove box, and a lithium-ion battery is assembled using an electrolyte, a metal lithium plate, a gasket, a spring and a button battery shell; the atmosphere in the glove box has an oxygen content and a water content of less than 0.1 ppm; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1.
[0039] The lithium-ion battery obtained by this method has a first discharge capacity of 4450mAh g at a charge and discharge current density of 0.1A / g. -1 , reversible charge capacity is 1221mAh g -1 After 30 cycles, the reversible specific capacity can still reach 812 mAh g -1 In terms of stability, the specific capacity did not decrease after 1500 cycles of charge and discharge at different currents (1.0, 10, 20, 25A / g). At a high current of 30A / g, it has a capacity of 205Wh kg electrode -1 Energy density is 63kWk gelectrode -1 High power density.
[0040] Example 3
[0041] A method for preparing a lithium ion battery negative electrode material based on hollow carbon nanocages comprises the following steps:
[0042] (1) sintering ammonium ferric citrate under inert gas at 750° C. for 3 h, cooling and treating in 1.5 mol / L hydrochloric acid at 65° C. for 15-20 h, filtering and drying to obtain carbon nanocages;
[0043] (2) dissolving carbon nanocages and PVDF in N-methylpyrrolidone at a mass ratio of 5:1, and grinding them thoroughly in an agate mortar to obtain a black slurry;
[0044] (3) The black slurry is evenly coated on the current collector, dried in an electric hot air drying oven at 80° C. for 12 h, and cut into carbon nanocage electrode pieces with a diameter of 10 mm using a commercially available manual slicer, and the pieces are punched for later use;
[0045] (4) The electrode plates are placed in a glove box, and a lithium-ion battery is assembled using an electrolyte, a metal lithium plate, a gasket, a spring and a button battery shell; the atmosphere in the glove box has an oxygen content and a water content of less than 0.1 ppm; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1.
[0046] The lithium-ion battery obtained by this method has a first discharge capacity of 4562 mAh g at a charge and discharge current density of 0.1 A / g. -1, reversible charge capacity is 1271mAh g -1 After 30 cycles, the reversible specific capacity can still reach 868 mAh g -1 In terms of stability, the specific capacity did not decrease after 1500 cycles of charge and discharge at different currents (1.0, 10, 20, 25A / g). At a high current of 30A / g, it has a capacity of 221Wh kg electrode -1 Energy density is 72kW k gelectrode -1 High power density.
[0047] Example 4
[0048] A method for preparing a lithium ion battery negative electrode material based on hollow carbon nanocages comprises the following steps:
[0049] (1) sintering ammonium ferric citrate under inert gas at 800° C. for 2 h, cooling and treating in 2 mol / L hydrochloric acid at 50° C. for 20 h, filtering and drying to obtain carbon nanocages;
[0050] (2) dissolving carbon nanocages and PVDF in N-methylpyrrolidone at a mass ratio of 5:1, and grinding them thoroughly in an agate mortar to obtain a black slurry;
[0051] (3) The black slurry is evenly coated on the current collector, dried in an electric hot air drying oven at 80° C. for 12 h, and cut into carbon nanocage electrode pieces with a diameter of 10 mm using a commercially available manual slicer, and the pieces are punched for later use;
[0052] (4) The electrode plates are placed in a glove box, and a lithium-ion battery is assembled using an electrolyte, a metal lithium plate, a gasket, a spring and a button battery shell; the atmosphere in the glove box has an oxygen content and a water content of less than 0.1 ppm; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1.
[0053] The lithium-ion battery obtained by this method has a first discharge capacity of 4551 mAh g at a charge and discharge current density of 0.1 A / g. -1 , reversible charge capacity is 1255mAh g -1 After 30 cycles, the reversible specific capacity can still reach 831 mAh g -1 In terms of stability, the specific capacity did not decrease after 1500 cycles of charge and discharge at different currents (1.0, 10, 20, 25A / g). At a maximum current of 30A / g, it has a capacity of 212Wh kg electrode -1 Energy density is 70kW k gelectrode-1 High power density.
[0054] Example 5
[0055] A method for preparing a lithium ion battery negative electrode material based on hollow carbon nanocages comprises the following steps:
[0056] (1) sintering ammonium ferric citrate under inert gas at 700° C. for 4 h, cooling and treating in 1 mol / L hydrochloric acid at 80° C. for 15 h, filtering and drying to obtain carbon nanocages;
[0057] (2) dissolving carbon nanocages and PVDF in N-methylpyrrolidone at a mass ratio of 5:1, and grinding them thoroughly in an agate mortar to obtain a black slurry;
[0058] (3) The black slurry is evenly coated on the current collector, dried in an electric hot air drying oven at 80° C. for 12 h, and cut into carbon nanocage electrode pieces with a diameter of 10 mm using a commercially available manual slicer, and the pieces are punched for later use;
[0059] (4) The electrode plates are placed in a glove box, and a lithium-ion battery is assembled using an electrolyte, a metal lithium plate, a gasket, a spring and a button battery shell; the atmosphere in the glove box has an oxygen content and a water content of less than 0.1 ppm; the electrolyte is a 1 mol / L LiPF6 solution, and the solvent is ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1.
[0060] The lithium-ion battery obtained by this method has a first discharge capacity of 4479 mAh g at a charge and discharge current density of 0.1 A / g. -1 , reversible charge capacity is 1231mAh g -1 After 30 cycles, the reversible specific capacity can still reach 811 mAh g -1 In terms of stability, the specific capacity did not decrease after 1500 cycles of charge and discharge at different currents (1.0, 10, 20, 25A / g). At a maximum current of 30A / g, it has a capacity of 202Wh kg electrode -1 Energy density is 64kW k gelectrode -1 High power density.
[0061] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0062] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nanocages, characterized in that: The following steps are involved: (1) sintering ammonium ferric citrate at high temperature under an inert gas, cooling, treating with acid, filtering, and drying to obtain carbon nanocages; (2) dissolving the carbon nanocages and the binder in N-methylpyrrolidone and grinding them thoroughly in an agate mortar to obtain a black slurry; (3) The black slurry is evenly coated on the current collector, and after drying, a carbon nanocage electrode plate is obtained, and the plate is punched for standby use; (4) The electrode plates are placed in a glove box, and the electrolyte, metal lithium plates, gaskets, springs and button cell shells are used to assemble a lithium-ion battery.
2. The method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nanocages according to claim 1, characterized in that: The high temperature sintering is sintering at 700-800° C. for 2-4 hours.
3. The method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nanocages according to claim 1, characterized in that: The acid treatment is carried out in 1-2 mol / L hydrochloric acid at 50-80° C. for 15-20 h.
4. The method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nanocages according to claim 1, characterized in that: The binder is PVDF.
5. The method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nanocages according to claim 1, characterized in that: The mass ratio of the carbon nano cage to the binder is 5:
1.
6. The method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nano cages according to claim 1, characterized in that: The current collector is copper foil or aluminum foil.
7. The method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nano cages according to claim 1, characterized in that: The drying is carried out in an electric hot air drying oven at 80° C. for 12 hours.
8. The method for preparing a negative electrode material for a lithium ion battery based on hollow carbon nanocages according to claim 1, characterized in that: The diameter of the carbon nanocage electrode plate is 10 mm.
9. The method for preparing a negative electrode material for a lithium-ion battery based on hollow carbon nanocages according to claim 1, characterized in that: The atmosphere of the glove box has an oxygen content and a water content both less than 0.1 ppm.