Organic-inorganic composite solid electrolyte isolating membrane, preparation method and semi-solid battery

By using a combination technology of a high heat-resistant organic polymer porous membrane and an inorganic solid electrolyte in semi-solid state batteries, a porous hybrid coating is formed and combined with the electrode through a hot pressing process, the strength of the composite solid electrolyte membrane in the prior art is solved. The problem of contacting the interface has achieved efficient lithium ion transmission and battery performance improvement, which is suitable for industrial applications.

CN119050604APending Publication Date: 2024-11-29中汽新能(天津)电池科技有限公司

Patent Information

Application Number
CN202411168146.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to achieve a composite solid electrolyte membrane with high strength, good conductivity and good interface contact in semi-solid state batteries, and the preparation process stability and industrialization are relatively difficult.

Method used

Using a porous organic polymer film with high heat resistance as the supporting substrate, the coating composition includes inorganic solid electrolyte, organic solid electrolyte and organic polymer binder. The porous hybrid coating is formed through the oily porous phase separation process and the hot pressing process is carried out. Combined with the electrodes to form efficient interface bonding.

Benefits of technology

It significantly improves the transmission capacity and battery performance of lithium ions, overcomes the fragility and interface resistance of traditional membranes, meets the high specific energy and safety requirements of semi-solid state batteries, and has the potential for large-scale industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050604A_ABST
    Figure CN119050604A_ABST
Patent Text Reader

Abstract

The invention discloses an organic-inorganic composite solid electrolyte isolating membrane and a preparation method thereof, and a semi-solid battery comprising the organic-inorganic composite solid electrolyte isolating membrane. The organic-inorganic composite solid electrolyte isolating membrane comprises a supporting substrate membrane and coatings on the two side surfaces of the supporting substrate membrane, the supporting basement membrane is a high-heat-resistance organic polymer porous membrane, the puncture strength of the supporting basement membrane is larger than or equal to 150 gf, the tensile strength of the supporting basement membrane is larger than or equal to 100 Mpa, the porosity of the supporting basement membrane is 50%-65%, and the pore size distribution interval is 50 nm-1 micron; the coating comprises an inorganic solid electrolyte, an organic solid electrolyte and an organic polymer binder. According to the present invention, the excellent physical strength of the separator, the good lithium ion transmission efficiency in the space structure of the separator, the excellent thermal safety performance, and the good interface contact between the electrode and the separator during the battery preparation are utilized, such that the electrical performance of the semi-solid state battery can be significantly improved, and the multifunctional requirement of the semi-solid state battery can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, in particular to an organic-inorganic composite solid electrolyte isolation membrane and a preparation method thereof, and a semi-solid battery comprising the organic-inorganic composite solid electrolyte isolation membrane. Background Art

[0002] In order to further improve the specific energy and safety of batteries, solid-state batteries have become the development trend of the industry. However, due to the environmental stability and cost issues of all-solid-state electrolytes, industrial applications are difficult. By effectively reducing the amount of liquid electrolyte, building a semi-solid battery system has become a necessary stage in the development of the current electrochemical system. Due to the extremely low injection volume of the semi-solid state, it is necessary to ensure that lithium ions have efficient transmission capabilities between the electrode and the separator, as well as in the spatial structure of the separator. The basic porosity of the traditional polyolefin separator substrate is about 50%, and the pore size distribution is between 30-50nm. At the same time, the superimposed coating will further reduce the ion conductivity of the polyolefin separator. At the same time, due to the low content of liquid electrolyte, solid electrolytes need to be added to the electrodes and separators to enhance the efficiency of lithium ion transmission, but the interface between the solid electrolyte and the electrode material presents a large number of solid-solid states, especially if the effective contact between the electrode and the separator is weak, which further deteriorates the transmission of ions between the positive and negative electrodes. In the existing technology, there are few composite solid electrolyte membranes that can simultaneously achieve high membrane strength (having a self-supporting base), greatly improve the interface performance between the electrode and the electrolyte membrane (having the bonding function between the electrode and the isolation membrane), and have good electrical conductivity.

[0003] For example, in the existing inorganic solid electrolyte technology, the inorganic solid electrolyte is transferred or coated with an electrode, and a solvent, a dispersant or a small amount of a binder is added to form an inorganic solid electrolyte membrane. The problem with this method is that the inorganic solid electrolyte membrane itself is relatively brittle, and the strength and flexibility are insufficient. Therefore, during the charge and discharge process of the electrode, it is easy to break or peel off, thereby degrading the performance and even causing safety problems in the contact between the positive and negative electrodes; secondly, the manufacturing stability and precision of this method are poor. Because the basic thickness of the positive electrode is in the order of ~100μm, there is inevitably a thickness difference on the surface. If the film is continuously coated on the electrode surface, it will bring about a significant difference in the thickness of the solid electrolyte membrane, causing surface inhomogeneity of lithium ion transmission and deteriorating performance. For example, CN 115763965B discloses an inorganic solid electrolyte membrane, which is obtained by coating a solid electrolyte LPSC mixed solvent on the electrode surface.

[0004] In the existing organic polymer solid electrolyte diaphragm or polymer composite technology, the organic-inorganic composite solid system combines the advantages of inorganic solid electrolyte and organic solid electrolyte, and the inorganic ceramic electrolyte mainly plays a filling role to improve mechanical strength and ionic conductivity. The polymer electrolyte has good processing and forming properties and is more suitable for large-scale mass production. In the technical solutions currently provided, most of them are blended with specific organic polymers and inorganic solid electrolytes in water or organic solvents, and the wet casting and drying film or transfer film is used to form a film. This method has the advantages of organic and inorganic to a certain extent, but the film thickness prepared by this method is still relatively high, basically in the order of tens of μm, and the supporting physical strength is still insufficient compared to the traditional porous membrane. For example, CN115966755A discloses a coated organic-inorganic composite solid electrolyte membrane with a porous membrane as the substrate. The purpose of this method is to form an organic-inorganic composite layer that is resistant to high voltage decomposition and has improved interface stability. Although this method can improve the flexibility of the coating itself, it does not form a strong effect between the solid electrolyte membrane and the interface, and has limited effect on reducing the interface resistance between the electrode and the electrolyte. In addition, this method is difficult to industrialize in practice because it involves processes such as secondary polymerization of polymers.

[0005] Therefore, it is urgent to propose a multifunctional separator for use in semi-solid battery systems. While having conventional physical and mechanical structures and chemical stability, it must also have good ionic conductivity. At the same time, under the premise of adding very little liquid electrolyte, it can form a good contact interface between the positive and negative electrodes to further improve the ion conduction capacity. More importantly, the preparation of this structure is easy to implement, with the potential for large-scale industrialization and stable and controllable industrial manufacturing. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies and defects of the prior art and to provide an organic-inorganic composite solid electrolyte separator and a preparation method thereof, and a semi-solid battery comprising the organic-inorganic composite solid electrolyte separator.

[0007] The first aspect of the present invention provides an organic-inorganic composite solid electrolyte isolation membrane, comprising a supporting base membrane and a coating on both sides of the supporting base membrane; the supporting base membrane is a highly heat-resistant organic polymer porous membrane, the puncture strength of the supporting base membrane is ≥150gf, the tensile strength is ≥100Mpa, the porosity is 50%-65%, and the pore size distribution range is 50nm-1μm; the components of the coating include an inorganic solid electrolyte, an organic solid electrolyte and an organic polymer binder.

[0008] The supporting base membrane uses a porous, macroporous polymer membrane as the supporting base to improve the mechanical strength of the isolation membrane structure and maximize the lithium ion transmission effect within a limited structure. At the same time, the polymer membrane uses a high heat-resistant material to effectively ensure the safety performance of the battery; the inorganic solid electrolyte can provide good ion conductivity under extremely low liquid electrolyte conditions, while improving the physical and mechanical strength and heat resistance of the isolation membrane; the organic solid electrolyte provides additional lithium ion conduction capability and gives the coating a certain flexibility, ensuring that microscopic deformation can be achieved when in contact with the electrode, which is conducive to microscopic interface contact; the organic polymer binder has a thermal bonding function and can effectively bond the isolation membrane to the electrode.

[0009] Preferably, the thickness of the supporting base film is 3.5 μm-20 μm, and the thickness of a single coating is 0.5 μm-3 μm.

[0010] Preferably, the supporting base film is one of polyimide, cellulose and PET.

[0011] Preferably, the thickness of the organic-inorganic composite solid electrolyte separator is no more than 23 μm, ensuring that the separator structure is light and thin to meet the basic indicator requirements of high specific energy of solid-state batteries.

[0012] Preferably, the inorganic solid electrolyte is an inorganic oxide solid electrolyte with a particle size of 100nm-700nm, including one or a mixture of two of the oxide solid electrolytes LATP and LLZO.

[0013] Preferably, the ionic conductivity of the inorganic solid electrolyte is 0.5 mS / cm-10 mS / cm.

[0014] Preferably, the organic solid electrolyte includes an organic polymer solid electrolyte, including one or a mixture of two or more of PEO, PVDF, PVDF-HFP, PEC, PPC, PAN, and PMMA.

[0015] Preferably, the organic polymer binder includes one or two of PVDF-HFP, PMMA, PI, and TPA.

[0016] The second aspect of the present invention provides a method for preparing an organic-inorganic composite solid electrolyte isolation membrane, characterized in that the method includes a coating composite slurry preparation process and a coating coating process for preparing the organic-inorganic composite solid electrolyte isolation membrane; the solvent used in the coating composite slurry preparation includes one of NMP, DMC, DMF, DMA, and DMSO, the coating composite slurry has a solid content of 30-50%, and a viscosity of 700-15000cps; the coating coating adopts an oily porogenic phase separation process. The oily porogenic phase separation process can ensure good bonding while forming a porous mixed coating.

[0017] The third aspect of the present invention provides a semi-solid-state battery, comprising the organic-inorganic composite solid electrolyte isolation membrane, wherein the positive electrode and the negative electrode of the battery are combined with the organic-inorganic composite solid electrolyte isolation membrane through a hot pressing process to form an interface-bonded battery electrode group.

[0018] By combining the positive and negative electrodes of the battery with an organic-inorganic composite solid electrolyte separator through a hot pressing process, a good interface contact effect between the electrode and the separator can be achieved, further improving the lithium ion conduction capability.

[0019] Among them, after obtaining the interface-bonded battery electrode group, a small amount of liquid electrolyte is added to obtain a semi-solid battery containing a multifunctional organic-inorganic composite solid electrolyte isolation membrane.

[0020] The positive electrode is an electrode prepared by various positive electrode active materials such as lithium iron phosphate, lithium cobalt oxide, ternary, lithium iron manganese phosphate, lithium-rich manganese-based, etc., in combination with a conductive agent, a binder, and a solid electrolyte.

[0021] The negative electrode is an electrode prepared by a single active material of silicon-carbon, silicon-oxygen or a mixed active material with graphite, a conductive agent, a binder, and a solid electrolyte, or a new negative electrode system such as a metal lithium negative electrode;

[0022] The hot pressing process preferably has the following conditions: 1Mpa-5Mpa, temperature 80°C-95°C, and time 30s-2min.

[0023] The semi-solid-state battery may be of a soft-pack, square or other type.

[0024] The organic-inorganic composite solid electrolyte separator of the present invention can significantly improve the electrical performance of semi-solid batteries by utilizing the excellent physical strength of the separator, good lithium ion transmission efficiency in the separator space structure, excellent thermal safety performance, and good interface contact between the electrode and the separator when preparing the battery, thereby overcoming the shortcomings of the prior art solutions that are difficult to balance performance and meeting the multifunctional requirements in semi-solid batteries.

[0025] At the same time, the implementation of this organic-inorganic composite solid electrolyte isolation membrane structure can cover some preparation processes and usage methods of traditional coating membranes, has a high mass production feasibility, and can promote the industrial application of high-energy-density and high-safety solid-state batteries more quickly. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of an organic-inorganic composite solid electrolyte isolation membrane according to an embodiment of the present invention.

[0027] Figure 2 It is a graph of the discharge capacity retention rates of Examples 1-6 of the present invention and Comparative Examples 1-2 at different discharge rates.

[0028] Figure 3 It is a comparison chart of the discharge capacity retention rates of Examples 1-6 of the present invention and Comparative Examples 1-2 at different charging rates.

[0029] Figure 4 It is a comparison chart of the discharge capacity retention rate of Examples 1-4 of the present invention and Comparative Examples 1-2 at room temperature and 2c cycle.

[0030] Description of reference numerals:

[0031] 10-supporting substrate film, 20-coating layer. DETAILED DESCRIPTION

[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] Example 1

[0034] (1) The supporting base membrane is a PI membrane with a porosity of 50%, a thickness of 17 μm, a puncture strength of 696 gf, and a tensile strength of 100 MPa.

[0035] (2) Pulping:

[0036] Take polymer solid electrolyte PEO and polymer binder PVDF-HFP in a ratio of 1:1 and disperse them in NMP, stir them thoroughly for 2 hours at a stirring speed of 1000r / min. After the dispersion is complete, add oxide solid electrolyte LATP with a particle size of 300nm to the above system, and then add cosolvent and surfactant and stir them thoroughly for 3 hours at a stirring speed of 1000r / min. The mass ratio of (PEO+PVDF-HFP slurry), LATP, cosolvent, and surfactant is 19:80:0.5:0.5.

[0037] (3) Coating:

[0038] Using a coating device, the coating slurry prepared in step (2) is applied to both sides of the PI base film in step (1), immersed in the first pure water coagulation bath for 40 seconds, and then immersed in the second pure water bath and the third pure water bath to clean the diaphragm; then dried in an oven at 70°C to obtain the organic-inorganic composite solid electrolyte coating isolation membrane, and the total thickness of the diaphragm membrane is 20 μm.

[0039] (4) Preparation of the lithium-ion battery assembled with the coating membrane:

[0040] The high nickel ternary positive electrode material is mixed with the conductive agent and the binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. The artificial graphite active particles, the conductive agent, and the binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is applied to the copper foil current collector and dried to obtain a negative electrode. The coated diaphragm is assembled with the prepared positive and negative electrodes into a finished soft-pack battery. After the liquid is injected and left to stand for 36-48 hours, the battery is hot-pressed in a hot press at a pressure of 1.2Mpa, a temperature of 90°C, and a time of 1min. After formation, a lithium-ion battery is prepared.

[0041] In step (2), the ratio of the organic solid electrolyte to the organic polymer binder is selected from 1:(1-3); the stirring time is selected from 1-5h; the stirring speed is selected from 500r / min-3000r / min; and the mass ratio of (PEO+PVDF-HFP slurry), LATP, co-solvent, and surfactant is selected from (10-40):(60-90):(0-1):(0-1).

[0042] The time of immersing in the first pure water coagulation bath in step (3) is selected from 20s to 100s.

[0043] Example 2

[0044] (1) The substrate is a cellulose membrane with a porosity of 60% and a thickness of 17 μm.

[0045] (2) Pulping:

[0046] Take polymer solid electrolyte PEO and polymer binder PVDF-HFP in a ratio of 1:1 and disperse them in NMP, stir them thoroughly for 2 hours at a stirring speed of 1000r / min. After the dispersion is complete, add oxide solid electrolyte LATP with a particle size of 300nm to the above system, and then add cosolvent and surfactant and stir them thoroughly for 3 hours at a stirring speed of 1000r / min. The mass ratio of (PEO+PVDF-HFP slurry), LATP, cosolvent, and surfactant is 19:80:0.5:0.5.

[0047] (3) Coating:

[0048] Using a coating device, the coating slurry prepared in step (2) is applied to both sides of the cellulose membrane in step (1), immersed in the first pure water coagulation bath for 40 seconds, and then immersed in the second pure water bath and the third pure water bath to clean the diaphragm; after drying in an oven at 70°C, the organic-inorganic composite solid electrolyte coating diaphragm is obtained, and the total thickness of the diaphragm is 20 μm.

[0049] (4) Preparation of the lithium-ion battery assembled with the coating membrane:

[0050] The high nickel ternary positive electrode material is mixed with the conductive agent and the binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. The artificial graphite active particles, the conductive agent, and the binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is applied to the copper foil current collector and dried to obtain a negative electrode. The coated diaphragm is assembled with the prepared positive and negative electrodes into a finished soft-pack battery. After the liquid is injected and left to stand for 36-48 hours, the battery is hot-pressed in a hot press at a pressure of 1.2Mpa, a temperature of 90°C, and a time of 1min. After formation, a lithium-ion battery is prepared.

[0051] Example 3

[0052] (1) The substrate selected is a PI membrane with a porosity of 50%, a thickness of 17 μm, a puncture strength of 696 gf, and a tensile strength of 100 MPa.

[0053] (2) Pulping:

[0054] Take polymer solid electrolyte PEO and polymer binder PVDF-HFP in a ratio of 1:1 and disperse them in NMP, stir them thoroughly for 2 hours at a stirring speed of 1000r / min. After the dispersion is complete, add oxide solid electrolyte LLZO with a particle size of 300nm to the above system, and then add cosolvent and surfactant and stir them thoroughly for 3 hours at a stirring speed of 1000r / min. The mass ratio of (PEO+PVDF-HFP slurry), LLZO, cosolvent, and surfactant is 19:80:0.5:0.5.

[0055] (3) Coating: Using a coating device, the coating slurry prepared in step (2) is applied to both sides of the PI base film in step (1), immersed in the first pure water coagulation bath for 40 seconds, and then immersed in the second pure water bath and the third pure water bath to clean the diaphragm. After drying in an oven at 70°C, the organic-inorganic composite solid electrolyte coating diaphragm is obtained, and the total thickness of the diaphragm is 20 μm.

[0056] (4) Preparation of the lithium-ion battery assembled with the coating diaphragm: The high-nickel ternary positive electrode material is mixed with the conductive agent and the binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. Artificial graphite active particles, conductive agent, and binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is applied to a copper foil current collector and dried to obtain a negative electrode. The coating diaphragm is assembled with the prepared positive and negative electrodes into a finished soft-pack battery. After the liquid is injected and left to stand for 36-48 hours, the battery is hot-pressed in a hot press at a pressure of 1.2Mpa, a temperature of 90°C, and a time of 1 minute. After formation, a lithium-ion battery is prepared.

[0057] Example 4

[0058] (1) The supporting base membrane is a PI membrane with a porosity of 50%, a thickness of 17 μm, a puncture strength of 696 gf, and a tensile strength of 100 MPa.

[0059] (2) Pulping:

[0060] Take polymer solid electrolyte PMMA and polymer binder PVDF-HFP in a ratio of 1:1 and disperse them in NMP, stir them thoroughly for 2 hours at a stirring speed of 1000r / min. After the dispersion is complete, add oxide solid electrolyte LLZO with a particle size of 300nm to the above system, and then add cosolvent and surfactant and stir them thoroughly for 3 hours at a stirring speed of 1000r / min. The mass ratio of (PMMA+PVDF-HFP slurry), LLZO, cosolvent, and surfactant is 19:80:0.5:0.5.

[0061] (3) Coating:

[0062] Using a coating device, the coating slurry prepared in step (2) is applied to both sides of the PI base film in step (1), immersed in the first pure water coagulation bath for 40 seconds, and then immersed in the second pure water bath and the third pure water bath for membrane cleaning. After drying in an oven at 70°C, the organic-inorganic composite solid electrolyte coating membrane is obtained, and the total thickness of the membrane is 20 μm.

[0063] (4) Preparation of the lithium-ion battery assembled with the coating membrane:

[0064] The high nickel ternary positive electrode material is mixed with the conductive agent and the binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. The artificial graphite active particles, the conductive agent, and the binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is applied to the copper foil current collector and dried to obtain a negative electrode. The coated diaphragm is assembled with the prepared positive and negative electrodes into a finished soft-pack battery. After the liquid is injected and left to stand for 36-48 hours, the battery is hot-pressed in a hot press at a pressure of 1.2Mpa, a temperature of 90°C, and a time of 1min. After formation, a lithium-ion battery is prepared.

[0065] Example 5

[0066] (1) The supporting base membrane is a PI membrane with a porosity of 50%, a thickness of 17 μm, a puncture strength of 696 gf, and a tensile strength of 100 MPa.

[0067] (2) Pulping:

[0068] Take polymer solid electrolyte PMMA and polymer binder TPA in a ratio of 1:1 and disperse them in NMP, stir them thoroughly for 2 hours at a stirring speed of 1000r / min. After complete dispersion, add oxide solid electrolyte LLZO with a particle size of 300nm to the above system, and then add cosolvent and surfactant and stir them thoroughly for 3 hours at a stirring speed of 1000r / min. The mass ratio of (PMMA+TPA slurry), LLZO, cosolvent, and surfactant is 19:80:0.5:0.5.

[0069] (3) Coating:

[0070] Using a coating device, the coating slurry prepared in step (2) is applied to both sides of the PI base film in step (1), immersed in the first pure water coagulation bath for 40 seconds, and then immersed in the second pure water bath and the third pure water bath for membrane cleaning. After drying in an oven at 70°C, the organic-inorganic composite solid electrolyte coating membrane is obtained, and the total thickness of the membrane is 20 μm.

[0071] (4) Preparation of the lithium-ion battery assembled with the coating membrane:

[0072] The high nickel ternary positive electrode material is mixed with the conductive agent and the binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. The artificial graphite active particles, the conductive agent, and the binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is applied to the copper foil current collector and dried to obtain a negative electrode. The coated diaphragm is assembled with the prepared positive and negative electrodes into a finished soft-pack battery. After the liquid is injected and left to stand for 36-48 hours, the battery is hot-pressed in a hot press at a pressure of 1.2Mpa, a temperature of 90°C, and a time of 1min. After formation, a lithium-ion battery is prepared.

[0073] Example 6

[0074] (1) The supporting base membrane is a PI membrane with a porosity of 50%, a thickness of 17 μm, a puncture strength of 696 gf, and a tensile strength of 100 MPa.

[0075] (2) Pulping:

[0076] Take polymer solid electrolyte PEO and polymer binder PVDF-HFP in a ratio of 1:1 and disperse them in NMP, stir them thoroughly for 2 hours at a stirring speed of 1000r / min. After the dispersion is complete, add oxide solid electrolyte LATP with a particle size of 300nm to the above system, and then add cosolvent and surfactant and stir them thoroughly for 3 hours at a stirring speed of 1000r / min. The mass ratio of (PEO+PVDF-HFP slurry), LATP, cosolvent, and surfactant is 19:80:0.5:0.5.

[0077] (3) Coating:

[0078] Using a coating device, the coating slurry prepared in step (2) is applied to both sides of the PI base film in step (1), immersed in the first pure water coagulation bath for 40 seconds, and then immersed in the second pure water bath and the third pure water bath for membrane cleaning. After drying in an oven at 70°C, the organic-inorganic composite solid electrolyte coating membrane is obtained, and the total thickness of the membrane is 20 μm.

[0079] (4) Preparation of the lithium-ion battery assembled with the coating membrane:

[0080] The high nickel ternary positive electrode material is mixed with the conductive agent and the binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. The artificial graphite active particles, the conductive agent, and the binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is applied to the copper foil current collector and dried to obtain a negative electrode. The coated diaphragm is assembled with the prepared positive and negative electrodes into a finished soft-pack battery. After the liquid is injected and left to stand for 36-48 hours, the battery is hot-pressed in a hot press at a pressure of 3Mpa, a temperature of 90°C, and a time of 30s. After formation, a lithium-ion battery is prepared.

[0081] Comparative Example 1

[0082] (1) The supporting base membrane is a PE membrane with a thickness of 16 μm, a porosity of 36%, a puncture strength of 445 gf, and a tensile strength of 100 MPa.

[0083] (2) Pulping:

[0084] Take 20% of LATP powder and 80% of deionized water and disperse them evenly to obtain a dispersion. Then take 80% of the dispersion, add 11% of a binder, 3.5% of a dispersant, 3.5% of a thickener and 2% of a wetting agent (wherein the binder is poly(methyl)acrylic acid, the dispersant is polyacrylate, the thickener is carboxymethyl cellulose, and the wetting agent is oxyethylene alkylphenol ether), mix and ball mill or sand mill for 3 hours, and obtain a coating slurry after filtering.

[0085] (3) Coating:

[0086] The coating slurry prepared in step (2) was coated on both sides of the base film of step (1) by using a coating device, and dried in an oven at 70° C. to obtain a coated diaphragm with a total thickness of 20 μm.

[0087] (4) Preparation of the lithium-ion battery assembled with the coating membrane:

[0088] The high nickel ternary positive electrode material is mixed with a conductive agent and a binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. Artificial graphite active particles, a conductive agent, and a binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is then coated on a copper foil current collector and dried to obtain a negative electrode. The coated separator is assembled with the prepared positive electrode, negative electrode, and electrolyte into a finished soft-pack battery, and a lithium-ion battery is prepared after formation.

[0089] Comparative Example 2

[0090] (1) The supporting base membrane is a PE membrane with a thickness of 16 μm, a porosity of 36%, a puncture strength of 445 gf, and a tensile strength of 100 MPa.

[0091] (2) Pulping:

[0092] Take 20% of the ceramic powder and 80% of deionized water and disperse them evenly to obtain a dispersion. Then take 80% of the dispersion, add 11% of the binder, 3.5% of the dispersant, 3.5% of the thickener and 2% of the wetting agent (wherein the binder is poly(methyl)acrylic acid, the dispersant is polyacrylate, the thickener is carboxymethyl cellulose, and the wetting agent is oxyethylene alkylphenol ether), mix and ball mill or sand mill for 3 hours, and obtain the coating slurry after filtering.

[0093] (3) Coating:

[0094] Using a coating device, the coating slurry prepared in step (2) is applied to both sides of the base film described in step (1), and after drying in an oven at 70°C, PVDF-HFP is sprayed on both sides of the diaphragm. After drying in an oven at 70°C, a coated diaphragm is obtained, and the total thickness of the diaphragm is 20 μm.

[0095] (4) Preparation of the lithium-ion battery assembled with the coating membrane:

[0096] The high nickel ternary positive electrode material is mixed with a conductive agent and a binder in a ratio of 97.8:1:1.2, and a certain amount of NMP is added as a solvent to form a slurry by stirring, which is then coated on an aluminum foil and vacuum dried at 90°C for 12 hours to obtain a positive electrode. Artificial graphite active particles, a conductive agent, and a binder are mixed in a ratio of 96.5:0.5:3 to prepare a slurry, which is then coated on a copper foil current collector and dried to obtain a negative electrode. The coated separator is assembled with the prepared positive electrode, negative electrode, and electrolyte into a finished soft-pack battery, and a lithium-ion battery is prepared after formation.

[0097] The performance of the diaphragms prepared in Examples 1-6 and Comparative Examples 1-3 was measured to determine the ion conductivity of the diaphragm, the bonding strength to the electrode sheet, the battery rate performance, and the battery cycle performance. The results are as follows:

[0098] 1. Physical and chemical testing of diaphragm

[0099] The test method for ion conductivity of the diaphragm is as follows:

[0100] The ion conductivity test was performed on the diaphragms prepared in Examples 1-6 and Comparative Examples 1-2, and a battery test cell tooling with 5 layers of diaphragms was assembled to perform an AC impedance test, and the resistance values ​​obtained from the test were linearly fitted, and the ion passing rate of the diaphragm was calculated. The test results are shown in Table 1.

[0101] The test method for the bonding strength between the diaphragm and the pole piece is as follows:

[0102] The hot-pressed batteries of Examples 1-6 and Comparative Examples 1-2 were disassembled, and samples of bonding of the positive electrode sheet and the separator were taken for bonding strength test. The test results are shown in Table 1.

[0103] Table 1

[0104]

[0105] The results show that the ion conductivity of the separator is: Example 1-6>Comparative Example 1>Comparative Example 2, and the separator-electrode bonding force is: Example 1-6>Comparative Example 2>Comparative Example 1. Comparative Example 1 has lithium ion conduction effect, and Comparative Example 2 has good interface bonding effect. The unique separator obtained by combining the advantages of the two embodiments 1-6 has not only high ion conductivity, but also high bonding property.

[0106] 2. Battery rate performance test

[0107] By performing charge and discharge tests at different rates of 1 / 5C, 1 / 3C, 1 / 2C, 1C, and 2C on Examples 1-6 and Comparative Examples 1-2, Figure 1 , 2 The discharge rates of different Figure 1 ) and different charging rates ( Figure 2 ), the results show that the capacity retention rate is in the order of Example 1-6>Comparative Example 1>Comparative Example 2, proving that the diaphragm can increase the transmission rate of lithium ions, thereby achieving rapid charge and discharge.

[0108] 3. Battery cycle performance test

[0109] By performing cycle tests on Examples 1-4 and Comparative Examples 1-2, Figure 3 The room temperature 2c cycle curve is shown; after 400 cycles, the capacity retention rate is as follows: Example 1-4>Comparative Example 1>Comparative Example 2. This proves that the coating material has good cycle stability and is conducive to a long battery life.

Claims

1. An organic-inorganic composite solid electrolyte isolation membrane, characterized in that: It comprises a supporting base membrane and a coating applied on both sides of the supporting base membrane; the supporting base membrane is a highly heat-resistant organic polymer porous membrane, the puncture strength of the supporting base membrane is ≥150gf, the tensile strength is ≥100Mpa, the porosity is 50%-65%, and the pore size distribution range is 50nm-1μm; the components of the coating include an inorganic solid electrolyte, an organic solid electrolyte and an organic polymer binder.

2. The organic-inorganic composite solid electrolyte isolation membrane according to claim 1, characterized in that: The thickness of the supporting base film is 3.5 μm-20 μm, and the thickness of a single coating is 0.5 μm-3 μm.

3. The organic-inorganic composite solid electrolyte isolation membrane according to claim 1, characterized in that: The supporting base film is one of polyimide, cellulose and PET.

4. The organic-inorganic composite solid electrolyte isolation membrane according to claim 1, characterized in that: The thickness of the organic-inorganic composite solid electrolyte isolation film is no more than 23 μm.

5. The organic-inorganic composite solid electrolyte separator according to claim 1, characterized in that: The inorganic solid electrolyte adopts an inorganic oxide solid electrolyte with a particle size of 100nm-700nm, including one or a mixture of two of the oxide solid electrolytes LATP and LLZO.

6. The organic-inorganic composite solid electrolyte isolation membrane according to claim 1, characterized in that: The ionic conductivity of the inorganic solid electrolyte is 0.5 mS / cm-10 mS / cm.

7. The organic-inorganic composite solid electrolyte separator according to claim 1, characterized in that: The organic solid electrolyte includes an organic polymer solid electrolyte, including one or a mixture of two or more of PEO, PVDF, PVDF-HFP, PEC, PPC, PAN, and PMMA.

8. The organic-inorganic composite solid electrolyte isolation membrane according to claim 1, characterized in that: The organic polymer binder includes one or two of PVDF-HFP, PMMA, PI and TPA.

9. A method for preparing an organic-inorganic composite solid electrolyte isolation membrane, characterized in that: Used for preparing the organic-inorganic composite solid electrolyte isolation membrane according to any one of claims 1 to 8, comprising a coating composite slurry preparation process and a coating coating process; the solvent used in preparing the coating composite slurry comprises one of NMP, DMC, DMF, DMA, and DMSO, the coating composite slurry has a solid content of 30-50% and a viscosity of 700-15000cps; The coating is applied using an oily porogenic phase separation process.

10. A semi-solid-state battery, characterized in that: The invention comprises the organic-inorganic composite solid electrolyte separator according to any one of claims 1 to 8, wherein the positive electrode and the negative electrode of the battery are combined with the organic-inorganic composite solid electrolyte separator through a hot pressing process to form an interface-bonded battery electrode group.

Citation Information

Patent Citations

  • Composite solid electrolyte membrane and preparation method thereof

    CN114335701A

  • Semi-solid sodium-ion battery diaphragm, preparation method thereof and semi-solid sodium-ion battery

    CN116780108A

  • Organic-inorganic composite coating diaphragm for lithium battery and preparation method of organic-inorganic composite coating diaphragm

    CN117096548A

Cited By

  • Diaphragm, preparation method thereof and battery

    CN119890615A

  • Separator, method for preparing the same, and battery

    CN119890615B

  • Diaphragm, secondary battery, battery pack and electronic equipment

    CN121394777A