Shielding film and folding electronic equipment
By designing a specific resistance change rate and material combination, the bending resistance of the electromagnetic shielding film is improved, and the problem of failure of the shielding film after multiple folds in the prior art is solved, thereby achieving higher bending times and better Blocking effect.
Patent Information
- Application Number
- CN202411169088.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The existing electromagnetic shielding film has poor bending resistance and is difficult to meet the performance requirements of folding electronic equipment, resulting in the shielding film failing after multiple folds.
Provide a shielding film, which satisfies a specific functional relationship between the resistance change rate of bending times and the difference between the bending times of bending times, adopts a shielding layer of materials such as aluminum, titanium, zinc, etc., and passes through a cover layer and glue layer. The design improves bending resistance.
It significantly improves the bending performance of the shielding film, extends its service life, meets the requirements of multiple folds, reduces the test cycle, and improves the shielding effect.
Smart Images

Figure CN119053145A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electromagnetic shielding, and in particular to a shielding film and a folding electronic device. Background Art
[0002] Electromagnetic shielding film can effectively prevent electromagnetic waves from harming the human body, and shield the interference of electromagnetic radiation on electronic equipment, ensuring the normal operation of electronic equipment. At the same time, by blocking the transmission of electromagnetic signals, it can also ensure that electronic information is not leaked or stolen.
[0003] With the development of communication equipment, foldable electronic devices (such as foldable mobile phones) have come into being. Applying the electromagnetic shielding film on the circuit board or soft board of the foldable electronic device can not only realize the folding of the foldable electronic device, but also avoid electromagnetic interference from the outside world and the foldable electronic device. After the foldable electronic device is folded many times, the electromagnetic shielding film will fail, and the higher the bending resistance of the electromagnetic shielding film, the lower the probability of failure. However, the bending resistance of the shielding film in the prior art is poor, and it is difficult to meet the performance requirements of foldable electronic devices. Therefore, it is urgent to improve the bending resistance of the shielding film. Summary of the invention
[0004] In view of this, the present invention provides a shielding film and a foldable electronic device to solve the problem in the related art that the shielding film is folded multiple times until the shielding film fails.
[0005] In the first aspect, the present invention provides a shielding film, wherein the number of bending times of the shielding film is within a first preset range, and the resistance change rate Δy of the shielding film and the difference Δx in the number of bending times of the shielding film satisfy the following function: 0.5≤|Δy*10000 / Δx|≤33; wherein Δy is the rate of change of resistance of the shielding film when it is bent for the mth time and the nth time, Δx is the difference between m and n, m is greater than n, and Δx is an integer multiple of 100, and the first preset range is 300-2000 times.
[0006] In an optional embodiment, the number of bending times of the shielding film is within a second preset range, and the shielding film resistance change rate Δy1 and the difference in the number of bending times of the shielding film Δx1| satisfy the following function: 0.1≤|Δy1*10000 / Δx1|≤20; wherein Δy1 is the rate of change of resistance of the shielding film when it is bent for the mth time and the nth time, Δx1 is the difference between m and n, m is greater than n, and Δx is an integer multiple of 100, and the first preset range is 2000-3500 times.
[0007] In an optional embodiment, the shielding film includes a shielding layer, and the material of the shielding layer is one or more of aluminum, titanium, zinc, iron, nickel, tungsten, chromium, cobalt, copper, silver, gold, ferrite, and carbon nanotubes.
[0008] In an optional embodiment, the thickness of the shielding layer is greater than 0.5% of the thickness of the shielding film.
[0009] In an optional implementation, it also includes:
[0010] Carrier layer;
[0011] A covering layer, located on one side surface of the carrier layer;
[0012] The shielding layer is located on a surface of the cover layer facing away from the carrier layer;
[0013] An adhesive layer, located on a surface of the shielding layer facing away from the covering layer;
[0014] A surface of the shielding layer on one side away from the covering layer has at least one protruding structure, and the protruding structure is embedded in or penetrates the adhesive layer.
[0015] In an optional implementation, the material of the covering layer includes polyimide, and the mass proportion of polyimide is 20%-80% of the covering layer.
[0016] In an optional embodiment, the covering layer has a thickness of 2 μm-20 μm.
[0017] In an optional embodiment, the thickness of the shielding film is 5 μm-30 μm, and the resistance value of the shielding film is 10 mΩ-1000 mΩ.
[0018] In an optional embodiment, a protective film is further included, which is located on a surface of the adhesive layer on a side away from the shielding layer.
[0019] In a second aspect, the present invention further provides a foldable electronic device, which adopts the shielding film of any embodiment of the first aspect.
[0020] The technical solution provided by the present invention has the following advantages:
[0021] 1. After the shielding film is bent, the resistance of the shielding film will change. Therefore, the resistance change of the shielding film is an important indicator to measure its bending performance. When the number of bending times of the shielding film is within a first preset range, and the shielding film resistance change rate Δy and the difference Δx of the shielding film bending times satisfy the following function: 0.5≤|Δy*10000 / Δx|≤33, the shielding film can achieve the set bending performance, so that the shielding film meets the requirements of multiple folding of foldable electronic devices. Since the first range is 300-2000 times, which is much smaller than the number of bending times at which the shielding film fails, the number of bending times of the shielding film is reduced, and the test cycle is reduced.
[0022] 2. When the number of bending times of the shielding film is within the second preset range, and the shielding film resistance change rate Δy1 and the difference in the number of bending times of the shielding film Δx1| satisfy the following function: 0.1≤|Δy1*10000 / Δx1|≤20, the bending performance of the shielding film is greater than the set bending performance, that is, the shielding film has better bending performance.
[0023] 3. The material of the shielding layer in the present invention is one or more of aluminum, titanium, zinc, iron, nickel, tungsten, chromium, cobalt, copper, silver, gold, ferrite, and carbon nanotubes to improve the shielding effect of the shielding layer.
[0024] 4. The present invention controls the content of polyimide in the covering layer to 20%-80%, thereby improving the bending property of the covering layer and the high temperature resistance of the covering layer, so that the covering layer has solder resistance, thereby improving the protective effect of the covering layer.
[0025] 5. The thickness of the covering layer of the present invention is 2 μm-20 μm, which can avoid solder corrosion while having high temperature resistance, and avoid the occurrence of faults in the covering layer and the shielding layer after multiple bending.
[0026] 6. The thickness of the shielding film in the present invention is 5 μm-30 μm. After the shielding film is applied to the circuit board or the flexible board, the circuit board or the flexible board can be bent 180°.
[0027] 7. In the shielding film provided by the present invention, the raised structure of the shielding layer is mainly used to pierce the adhesive layer to achieve grounding of the shielding layer, thereby being able to lead out the charge accumulated in the adhesive layer to improve the shielding effect of the shielding film. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 is a schematic structural diagram of a shielding film according to an embodiment of the present invention;
[0030] Figure 2 is a side cross-sectional view of a shielding film according to an embodiment of the present invention;
[0031] Figure 3 is a side cross-sectional view of another shielding film according to an embodiment of the present invention.
[0032] Description of reference numerals:
[0033] 1. Carrier layer; 2. Covering layer; 3. Shielding layer; 31. Raised structure; 4. Adhesive layer; 5. Protective layer. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It is understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only some structures related to the present invention are shown in the accompanying drawings, rather than all structures. In the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention. Various structural schematic diagrams according to embodiments of the present invention are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified for the purpose of clear expression, and some details may be omitted. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships between them are only exemplary, and may be deviated due to manufacturing tolerances or technical limitations in practice, and those skilled in the art may additionally design regions / layers with different shapes, sizes, and relative positions according to actual needs. In the context of the present invention, when a layer / element is referred to as being "on" another layer / element, the layer / element may be directly on the other layer / element, or there may be an intermediate layer / element between them. In addition, if one layer / element is "on" another layer / element in one orientation, then when the orientation is reversed, the layer / element may be "below" the other layer / element.
[0035] The shielding film provided by the present invention has a bending number of the shielding film within a first preset range, and the shielding film resistance change rate Δy and the shielding film bending number difference Δx satisfy the following function: 0.5≤|Δy*10000 / Δx|≤33; wherein Δy is the resistance change rate of the shielding film when it is bent for the mth time and the nth time, Δx is the difference between m and n, m is greater than n, and Δx is an integer multiple of 100, and the first preset range is 300-2000 times. After the shielding film is bent, the resistance of the shielding film will change, so the resistance change of the shielding film is an important indicator for measuring its bending performance. When the shielding film is bent for the first preset range, and the shielding film resistance change rate Δy and the shielding film bending number difference Δx satisfy the following function: 0.5≤|Δy*10000 / Δx|≤33, the shielding film can achieve the set bending performance, so that the shielding film meets the requirements of multiple folding of foldable electronic devices. Since the first range is 300-2000 times, which is much less than the number of bending times at which the shielding film fails, the number of bending times of the shielding film is reduced, and the test cycle is reduced. In addition, it should be noted that the value of |Δy*10000 / Δx| can be one of 0.6, 0.7, 0.8, 1.0, 1.2, 1.5, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, 15.0, 18.0, 20.0, 23.0, 25.0, 28.0, 30.0, 31.0, and 32.0.
[0036] The shielding film provided by the present invention has a bending number within a second preset range, and the shielding film resistance change rate Δy1 and the shielding film bending number difference Δx1 satisfy the following function: 0.1≤|Δy1*1000 / Δx1|≤20; wherein Δy1 is the change rate of the shielding film resistance when the shielding film is bent for the mth time and the nth time, and Δx1 is the difference between m and n, m is greater than n, and Δx is an integer multiple of 100, and the first preset range is 2000-3500 times. When the shielding film is bent for the second preset range, and the shielding film resistance change rate Δy1 and the shielding film bending number difference Δx1 satisfy the following function: 0.1≤|Δy1*10000 / Δx1|≤20, the shielding film has a bending performance greater than the set bending performance, that is, the shielding film has a better bending performance. It should be noted that the value of |Δy1*10000 / Δx1| can be one of 0.3, 0.5, 0.8, 1.0, 1.5, 1.8, 2.0, 3.0, 5.0, 8.0, 10.0, 13.0, 15.0, 18.0, and 19.0.
[0037] In the present invention, the resistance change rate Δy is calculated as Δy=(y m -y n ) / y n, where y m is the resistance value of the shielding layer 3 after multiple bending, y n The original resistance value of the shielding layer 3 before multiple bending.
[0038] like Figures 1 to 3 As shown, the present invention provides a shielding film, which includes but is not limited to a carrier layer 1, a covering layer 2, a shielding layer 3 and an adhesive layer 4.
[0039] In this embodiment, the carrier layer 1 uses a PET (Polyethylene terephthalate) release carrier film. Of course, in other embodiments, film materials of other materials can also be used as carriers. Optionally, the carrier film can be a bisphenol A type epoxy resin, an acrylic resin, or a polyester resin. In addition, the resin used can also be selected from epoxy resin, cyanate resin, polyphenylene ether resin, polybutadiene resin, butadiene resin, bismaleimide-triazine resin (BT), bismaleimide resin, polytetrafluoroethylene resin, polyimide resin, phenolic resin, acrylic resin, liquid crystal resin, benzoxazine resin, phenoxy resin, nitrile rubber, carboxyl-terminated nitrile rubber or hydroxy-terminated nitrile rubber, any one or a mixture of at least two of them, but not limited to this, and all resin materials disclosed in the prior art can be used. The mixture is, for example, a mixture of epoxy resin and cyanate resin, a mixture of polyphenylene oxide resin and polybutadiene resin, a mixture of styrene butadiene resin and BT resin, a mixture of polytetrafluoroethylene resin and polyimide resin, a mixture of phenolic resin and acrylic resin, a mixture of epoxy resin, cyanate resin and polyphenylene oxide resin, a mixture of polybutadiene resin, styrene butadiene resin and BT resin, a mixture of polytetrafluoroethylene resin, polyimide resin, phenolic resin and acrylic resin. That is, a mixture of two or more resins can be used. The resin used in the covering layer 2 and the adhesive layer 4 includes the resin material used in the carrier layer 1, that is, the resin used in the covering layer 2 and the adhesive layer 4 can use the resin type used in the carrier layer 1. Among them, the resins used between the carrier layer 1, the covering layer 2, and the adhesive layer 4 can be the same or different from each other.
[0040] It should be noted that the covering layer 2 may have insulating properties and can support the shielding layer 3; the covering layer 2 may also be a structure containing conductive particles and has a certain conductive function, which can improve the shielding effect together with the shielding.
[0041] In another embodiment, the shielding film may only consist of the shielding layer 3 and the adhesive layer 4, and the shielding layer 3 is stacked on one surface of the adhesive layer 4. The shielding film with the above structure also has a good shielding effect.
[0042] It should be noted that the carrier layer 1, the cover layer 2, the shielding layer 3 and the adhesive layer 4 in the above embodiment can be a single-layer structure or a multi-layer structure. When it is a multi-layer structure, the materials used between the layers can be the same or different.
[0043] The covering layer 2 is located on one side surface of the carrier layer 1 , the shielding layer 3 is located on one side surface of the covering layer 2 facing away from the carrier layer 1 , and the adhesive layer 4 is located on one side surface of the shielding layer 3 relative to the covering layer 2 .
[0044] like Figure 1 As shown, the PET release carrier film in the shielding film is arranged at the bottom, the covering layer 2 is attached to the upper surface of the PET release carrier film, the shielding layer 3 is attached to the upper surface of the covering layer 2, and the adhesive layer 4 is attached to the upper surface of the shielding layer 3.
[0045] In some optional embodiments, such as Figure 1 As shown, the surface of the shielding layer 3 facing away from the cover layer 2 has a plurality of protrusion structures 31, and the protrusion structure 31 is spike-shaped. As an alternative embodiment, the protrusion structure 31 can also be truncated. The adhesive layer 4 is connected to the pad line, and the pad line is grounded. Figure 2 As shown, part of the protruding structure 31 is embedded in the adhesive layer 4. As an alternative embodiment, Figure 3 The part of the raised structure 31 shown can also penetrate the adhesive layer 4, thereby realizing the grounding of the shielding layer 3, so that the shielding layer 3 can conduct the charge accumulated in the adhesive layer 4, thereby improving the shielding effect of the shielding film. The raised structure 31 can also contact the conductive particles in the adhesive layer 4. During the bending process, the raised structure 31 has a buffering effect on the conductive particles, reducing the stress of the conductive particles on the shielding layer 3, avoiding the fracture of the shielding layer 3 due to stress concentration caused by multiple bending, and extending the service life of the shielding layer 3, thereby extending the service life of the shielding film.
[0046] In an alternative embodiment, the surface of the shielding layer 3 facing away from the cover layer 2 has one protruding structure 31 or a plurality of protruding structures 31 .
[0047] In some optional embodiments, the material of the shielding layer 3 is made of one of titanium, zinc, iron, nickel, tungsten, chromium, cobalt, copper, silver, gold, ferrite, and carbon nanotubes. Or the shielding layer 3 is an alloy formed by at least two of aluminum, titanium, zinc, iron, nickel, tungsten, chromium, cobalt, copper, silver, gold, ferrite, and carbon nanotubes. This embodiment is not specifically limited here and is determined according to actual product design requirements.
[0048] Specifically in this embodiment, the shielding layer 3 is made of copper, which has low cost, can ensure the grounding channel and shielding effect, and improve the overall shielding effect of the electromagnetic shielding film, so as to improve the bending resistance of the shielding layer 3.
[0049] The shielding film provided in this embodiment has high bending resistance, can have good adaptability on a flexible board or a folding circuit board, meets the high-frequency folding performance requirements of the flexible board, and has a low probability of failure.
[0050] In some optional embodiments, the thickness of the shielding layer 3 is greater than 0.5% of the thickness of the shielding film, that is, the minimum thickness of the shielding layer 3 is 0.02 μm. The thickness of the shielding layer 3 can be set according to specific requirements and will not be further elaborated here.
[0051] In some optional embodiments, the material of the covering layer 2 is polyimide, and the mass proportion of polyimide is 20%-80% of the covering layer 2, for example, 20%, 30%, 55%, 79%, 80%; when the mass proportion of polyimide in the covering layer 2 is greater than 80%, the covering layer 2 becomes rigid, and after multiple bending, the covering layer 2 and the shielding layer 3 are faulted, which reduces the bending resistance of the shielding film. When the content of polyimide in the covering layer 2 is less than 20%, the high temperature resistance of the covering layer 2 is reduced. When the shielding film is attached to the surface of the folding electronic device or the soft board, the covering layer 2 is easily burned by the high temperature of the solder, causing the shielding film to fail, thereby causing the color change and failure of the circuit board or the soft board. In this embodiment, the mass proportion of polyimide in the covering layer 2 is controlled to 20%-80%, and the high temperature resistance of the covering layer 2 is improved while improving the bending shape of the covering layer 2, so that the covering layer 2 has a solder-resistant shape to improve the protective effect of the covering layer 2.
[0052] In some optional embodiments, the thickness of the covering layer 2 is between 2 μm and 20 μm, such as 2 μm, 3 μm, 5 μm, 10 μm, 19 μm, and 20 μm. When the thickness of the covering layer 2 is less than 2 μm, the high temperature resistance of the covering layer 2 is reduced, and solder corrosion will occur, directly leading to failure or damage of the shielding effectiveness. When the thickness of the covering layer 2 is greater than 20 μm, the covering layer 2 and the shielding layer 3 will be faulted after the shielding film is bent multiple times. In addition, the thickness of the covering layer 2 will cause the overall structure of the shielding film to be thicker and higher, which is not conducive to the 180° bending of the folded circuit board or the flexible board.
[0053] In some optional embodiments, the thickness of the shielding film is 5 μm-30 μm, such as 5 μm, 6 μm, 10 μm, 20 μm, 23 μm, 30 μm, and the resistance value of the shielding film is 10 mΩ-1000 mΩ.
[0054] In some optional embodiments, a protective film is further included, which is located on a surface of the adhesive layer 4 that is away from the shielding layer 3 .
[0055] In a second aspect, the present embodiment also includes a foldable electronic device, which includes the shielding film in any embodiment.
[0056] In this solution, when the shielding film meets the formula within the first preset range, the shielding film has better bending resistance; when the shielding film meets the formula within the second preset range, the shielding film has better bending resistance. In order to better illustrate the technical effect of the present invention, samples that partially meet the formula within the first preset range, the formula within the second preset range, and samples that do not meet the above formulas are subjected to full-cycle bending tests, and the grounding effect after bending is tested.
[0057] Example 1
[0058] A shielding film, the shielding film is composed of a carrier layer 1, a covering layer 2, a shielding layer 3 and an adhesive layer 4, the covering layer 2 is located on one side surface of the carrier layer 1; the shielding layer 3 is located on the side surface of the covering layer 2 away from the carrier layer 1;
[0059] The adhesive layer 4 is located on one surface of the cover layer 2 and opposite to the carrier layer 1; the shielding film satisfies |Δy*10000 / Δx|=0.6.
[0060] The above samples were tested, and the test results showed that the shielding film's bending resistance can reach more than 2,500 times.
[0061] Example 2
[0062] A shielding film, the shielding film is composed of a carrier layer 1, a covering layer 2, a shielding layer 3 and an adhesive layer 4, the covering layer 2 is located on one side surface of the carrier layer 1; the shielding layer 3 is located on the side surface of the covering layer 2 away from the carrier layer 1;
[0063] The adhesive layer 4 is located on one surface of the cover layer 2 and opposite to the carrier layer 1; the shielding film satisfies |Δy*10000 / Δx|=32.8.
[0064] The above samples were tested, and the test results showed that the shielding film had a bending resistance of more than 2,500 times.
[0065] Example 3
[0066] A shielding film, the shielding film is composed of a carrier layer 1, a covering layer 2, a shielding layer 3 and an adhesive layer 4, the covering layer 2 is located on one side surface of the carrier layer 1; the shielding layer 3 is located on the side surface of the covering layer 2 away from the carrier layer 1;
[0067] The adhesive layer 4 is located on one surface of the cover layer 2 and the carrier layer 1; the shielding film satisfies |Δy*10000 / Δx|=9.0.
[0068] The above samples were tested, and the test results showed that the shielding film had a bending resistance of more than 2,800 times.
[0069] Example 4
[0070] In addition to satisfying the conditions of Embodiment 3, the shielding film of this embodiment further satisfies |Δy1*10000 / Δx1|=0.2.
[0071] The above samples were tested, and the test results showed that the shielding film's bending resistance can reach more than 4,000 times.
[0072] Example 5
[0073] In addition to satisfying the conditions of Embodiment 3, the shielding film of this embodiment further satisfies |Δy1*10000 / Δx1|=20.0.
[0074] The above samples were tested, and the test results showed that the shielding film's bending resistance can reach more than 4,000 times.
[0075] Comparative Example 1
[0076] In this embodiment, except that the formula within the first preset range is not satisfied and the adhesive layer 4 only contains conductive particles but no protruding structures 31 , the other conditions are all combined.
[0077] The comparative example was tested, and the test results showed that the bending resistance of the shielding film could reach 1171 times, that is, the sample had very poor bending resistance and could not meet the application requirements of the shielding film with high bending resistance.
[0078] It can be seen from Examples 1-5 and the comparative example that the shielding film satisfying the functional relationship of the present application has better bending resistance than conventional shielding films, and the bending resistance can reach more than 2,500 times, or even up to 15,000 times.
[0079] In the present invention, the bending test method is: pressing the shielding film sample with a 25-micron-thick polyimide film (pressing conditions: pre-pressing time 10 seconds, molding time 180 seconds, the mass of the weight provided for pressing is 120 kg, and the pressing temperature is 185°C); baking and curing after pressing (baking temperature 160°C, baking time 90 minutes). The width of the shielding film after pressing is 1.5 cm, the length is 15 cm, the bending conditions are R angle 0.38 mm, speed 150 rpm, angle ±135°, and the mass of the pressure weight is 500 g.
[0080] In addition, when using the above bending test method to compare the bending resistance of different shielding films, when the shielding film on-resistance is greater than 50% of the initial value before the shielding film is bent, the test is stopped and the number of bends is recorded.
[0081] In the above description, the technical details of the patterning and etching of each layer are not described in detail. However, those skilled in the art should understand that various technical means can be used to form layers, regions, etc. of desired shapes. In addition, in order to form the same structure, those skilled in the art can also design methods that are not completely the same as the methods described above. In addition, although the various embodiments are described above separately, this does not mean that the measures in the various embodiments cannot be used in combination to advantage.
[0082] In the description of this specification, the description with reference to the terms "this embodiment", "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0083] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0084] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0085] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0086] Although the embodiments of the present invention have been described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.
Claims
1. A shielding film, characterized in that: The number of bending times of the shielding film is within a first preset range, and the shielding film resistance change rate Δy and the difference Δx in the number of bending times of the shielding film satisfy the following function: 0.5≤|Δy*10000 / Δx|≤33; wherein Δy is the rate of change of resistance of the shielding film when it is bent for the mth time and the nth time, Δx is the difference between m and n, m is greater than n, and Δx is an integer multiple of 100, and the first preset range is 300-2000 times.
2. The shielding film according to claim 1, characterized in that The number of bending times of the shielding film is within the second preset range, and the shielding film resistance change rate Δy1 and the difference Δx1 in the number of bending times of the shielding film satisfy the following function: 0.1≤|Δy1*10000 / Δx1|≤20; wherein Δy1 is the rate of change of resistance of the shielding film when it is bent for the mth time and the nth time, Δx1 is the difference between m and n, m is greater than n, and Δx is an integer multiple of 100, and the second preset range is 2000-3500 times.
3. The shielding film according to claim 1 or 2, characterized in that: The shielding film comprises a shielding layer (3), and the material of the shielding layer (3) is one or more of aluminum, titanium, zinc, iron, nickel, tungsten, chromium, cobalt, copper, silver, gold, ferrite, and carbon nanotubes.
4. The shielding film according to claim 3, characterized in that The thickness of the shielding layer (3) is greater than 0.5% of the thickness of the shielding film.
5. The shielding film according to claim 4, characterized in that Also includes: Carrier layer (1); A covering layer (2) is located on one side surface of the carrier layer (1); The shielding layer (3) is located on a surface of the cover layer (2) that is away from the carrier layer (1); An adhesive layer (4) is located on a surface of the shielding layer (3) that is away from the covering layer (2); A surface of the shielding layer (3) on one side facing away from the covering layer (2) has at least one protruding structure (31), and the protruding structure (31) is embedded in or penetrates the adhesive layer (4).
6. The shielding film according to claim 5, characterized in that The material of the covering layer (2) includes polyimide, and the mass proportion of the polyimide is 20%-80% of the mass of the covering layer (2).
7. The shielding film according to claim 5, characterized in that The thickness of the covering layer (2) is 2 μm-20 μm.
8. The shielding film according to claim 5, characterized in that The thickness of the shielding film is 5 μm-30 μm, and the resistance value of the shielding film is 10 mΩ-1000 mΩ.
9. The shielding film according to claim 5, characterized in that It also includes a protective film, which is located on the surface of the adhesive layer (4) on the side facing away from the shielding layer (3).
10. A foldable electronic device, characterized in that: A shielding film as described in any one of claims 1 to 9 is used.