Catalyst and method for manufacturing the same
By using glycerol and oxalic acid instead of ethylene glycol in the polyol method, controlling the shape and size of the metal nanostructures, the problem of poor catalyst performance and durability in the prior art is solved, and a high suitable for fuel cells and water electrolysis is provided. Performance catalyst.
Patent Information
- Application Number
- CN202480002232.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2024-03-14
- Publication Date
- 2024-11-29
AI Technical Summary
When using ethylene glycol as a reducing agent in the existing polyol method, it is difficult to control the shape and size of the metal nanostructure, resulting in poor performance and durability of the catalyst in fuel cell and water electrolysis applications.
Glycerin is used instead of ethylene glycol and oxalic acid is used as a reducing additive to prepare metal nanostructures on carbon carriers. By controlling the ratio and reaction conditions of glycerol and oxalic acid, the shape and size of metal nanostructures are achieved.
The uniformity of the shape and size of the catalyst is achieved, the performance and durability of the catalyst is improved, and it is suitable for fuel cell and water electrolysis applications.
Smart Images

Figure CN119053383A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to catalysts and methods for making the same. Background Art
[0002] As a method for producing a metal nanostructure and a catalyst including the same, a "polyol method" is known.
[0003] In the "polyol method", a polyol is used as a reducing agent, a metal salt precursor is reduced to prepare a metal nanostructure, and the fabricated metal nanostructure is supported on a carbon-based support.
[0004] A representative example of the “polyol” used in the polyol method is ethylene glycol, which has a dual function as a solvent and a reducing agent.
[0005] Ethylene glycol has the advantages of low viscosity and excellent reactivity, but has the following disadvantages: it is difficult to handle due to its strong toxicity and high water solubility, and its ability to uniformly control the shape and size of metal nanostructures to uniformly distribute the metal nanostructures is limited. Summary of the invention
[0006]
Technical issues
[0007] Embodiments have been made to solve the problem of using ethylene glycol as a "polyol".
[0008]
Technical solution
[0009] In an embodiment, glycerol is used instead of ethylene glycol as the "polyol", and oxalic acid is used as the "reduction aid" for the polyol reaction.
[0010]
Technical Effect
[0011] In an embodiment, under the condition where glycerol and oxalic acid coexist, the shape and size of the metal nanostructure are easily controlled, and at the same time, the metal nanostructure having the controlled shape and size is supported on a carbon-based support to prepare a catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 A schematic reaction scheme of a method of manufacturing a metal nanostructure according to an embodiment is explained. DETAILED DESCRIPTION
[0013] Advantages and features of the present disclosure and methods of achieving the same will become apparent from the embodiments described in detail with the accompanying drawings. However, the embodiments may not be limited to the embodiments disclosed below.
[0014] (Definition of terminology)
[0015] Unless otherwise defined, all terms (including technical terms and scientific terms) used in this specification have the same meaning as those generally understood by those skilled in the art. Further, unless otherwise defined, all terms defined in commonly used dictionaries may be interpreted undesirably or exaggeratedly.
[0016] Throughout this specification, unless explicitly described to the contrary, “comprising” any component will be understood to imply the further inclusion of other components rather than the exclusion of any other components. In addition, unless the context clearly indicates otherwise, the singular form is intended to include the plural form.
[0017] In the present specification, the “particle size” or “average particle size” can be measured by a method well known to those skilled in the art, and for example, can be measured by a particle size analyzer or by a transmission electron microscope or a scanning electron microscope.
[0018] (Method for producing catalyst)
[0019] Generally, the catalyst is manufactured by fabricating a metal nanostructure using ethylene glycol and supporting the metal nanostructure on a carbon-based support.
[0020] However, ethylene glycol is not only difficult to handle due to its strong toxicity and high water solubility, but also has limited ability to control the shape and size of metal nanostructures. In particular, when the catalyst including the metal nanostructure is used as a catalyst for a fuel cell monomer or a catalyst for water electrolysis, the limited ability of ethylene glycol to control the shape and size of the metal nanostructure is problematic.
[0021] Specifically, when the shape and size of the metal nanostructure are non-uniform or large, the metal nanostructure may be dissolved from the catalyst, which may damage the polymer electrolyte membrane, and may deteriorate the performance and durability of a fuel cell cell or a water electrolysis device.
[0022] In an embodiment, glycerol is used instead of ethylene glycol as the "polyol", and oxalic acid is used as the "reduction aid" for the polyol reaction.
[0023] Specifically, the embodiment provides a method of manufacturing a catalyst, the method including reacting an aqueous precursor solution including a metal salt, glycerol, and oxalic acid in the presence of a carbon-based support.
[0024] More specifically, in an embodiment, under the condition where glycerol and oxalic acid coexist, the shape and size of the metal nanostructure are easily controlled, and the metal nanostructure with the controlled shape and size is loaded on a carbon-based carrier to prepare a catalyst. The process of manufacturing the metal nanostructure and the process of loading the metal nanostructure on the carbon-based carrier are performed in situ.
[0025] Since a metal nanostructure having a controlled shape and size is supported on a carbon-based carrier, an embodiment can provide a catalyst having excellent performance and durability. In particular, the catalyst is suitable for use as a catalyst for a fuel cell monomer or a catalyst for water electrolysis.
[0026] Hereinafter, raw materials for a catalyst and a method of manufacturing a catalyst using the raw materials according to an embodiment will be described in detail.
[0027] Metal Salts
[0028] Metal salts are precursors of metal nanostructures.
[0029] The metal constituting the metal salt may be a noble metal, a transition metal, an alloy thereof or a mixture thereof. Specifically, the noble metal may include platinum (Pt), ruthenium (Ru), osmium (Os), iridium (Ir), palladium (Pd), an alloy thereof or a mixture thereof, and may be, for example, platinum. In addition, the transition metal may include cobalt (Co), iron (Fe), nickel (Ni), zinc (Zn), tin (Sn), manganese (Mn), copper (Cu), scandium (Sc), titanium (Ti), vanadium, (V), chromium (Cr), zirconium (Zr), yttrium (Y), niobium (Nb), an alloy thereof or a mixture thereof.
[0030] Meanwhile, the metal salt is in the form of a salt, and may include nitrate, sulfate, acetate, chloride, oxide, or a combination thereof of a metal.
[0031] Specifically, the metal salt is a metal salt including platinum (Pt), and may be dinitro-diamine platinum nitrate, chloroplatinic acid, potassium chloroplatinate, platinum oxalate, monoethanolamine platinum hydroxide, triethanolamine platinum hydroxide, or a combination thereof.
[0032] For example, the metal salt may be dinitro-diamine platinum nitrate. As a more specific example, the dinitro-diamine platinum nitrate may be an alkaline platinum precursor such as (TEA)-2Pt(OH)6, (MEA)-2Pt(OH)6, [Pt(NH3)4]Cl2, [Pt(NH3)4](NO3)2, [Pt(NH3)4](OH)2, Pt(NH3)2Cl2 or (NH4)2[PtCl4].
[0033] glycerin
[0034] Glycerin is a polyol compound and is represented by the following Chemical Formula 1:
[0035] [Chemical formula 1]
[0036]
[0037] Glycerol, a byproduct of biodiesel, can be purchased easily and cheaply industrially and is less toxic than ethylene glycol, and is therefore used as a food additive.
[0038] Theoretically, since glycerol is a polyol compound, glycerol can be used as a solvent and a reducing agent for reducing the metal salt.
[0039] However, the polyol used in the "polyol process" needs to have a low viscosity. Since glycerol has a relatively high viscosity compared to ethylene glycol, glycerol has not been processed in the "polyol process" so far.
[0040] In an embodiment, in order to reduce the viscosity of glycerol, glycerol is dissolved in water and used in the form of an aqueous solution. Specifically, a precursor aqueous solution including a metal salt, glycerol and oxalic acid is reacted. More details about this will be described below.
[0041] At the same time, glycerol acts as a template and can make the shape and size uniform during the process of converting the metal salt into the metal nanostructure. As a result, by using glycerol, the metal nanostructure can be uniformly distributed.
[0042] oxalic acid
[0043] Oxalic acid can assist the reducing function of glycerol in the process of converting the metal salt into the metal nanostructure while maintaining the pH of the reaction between the metal salt and glycerol. In this sense, oxalic acid acts as a "reducing aid".
[0044] Specifically, the precursor aqueous solution including the metal salt, glycerol and oxalic acid may further include formic acid. Here, the formic acid may be converted from a part of the oxalic acid.
[0045] The molar ratio of the metal salt to the oxalic acid may be 1:0.5 to 1:12, specifically 1:3 to 1:10, more specifically 1:4 to 1:9, and for example, 1:5 to 1:7. Within such a range, the effects of oxalic acid as a pH adjustment and reduction aid may be improved.
[0046] Carbon Support
[0047] The support may be a carbon-based support.
[0048] The carbon-based support may include carbon black, graphite, carbon nanofiber, graphitized carbon nanofiber, carbon nanotube, carbon nanohorn, carbon nanowire or a combination thereof. Carbon black may include, for example, Denka black, Ketjen black, acetylene black, channel black, furnace black, lamp black, thermal black or a combination thereof.
[0049] The specific surface area of carbon carriers can be 250m 2 / g to 1,200m 2 / g. When the specific surface area of the carbon carrier is 250m 2 / g or more, the area attached to the metal nanostructure can be increased, and the effective surface area can be increased by dispersing the metal nanostructure at a high level. At the same time, in which the specific surface area of the carbon-based carrier is greater than 1,200 m 2 / g, when an electrode for a fuel cell is formed, the presence rate of ultrafine pores (less than about 20 angstroms) that are difficult for ion exchange resins to penetrate increases, which can reduce the utilization efficiency of the catalyst.
[0050] The precursor aqueous solution including the metal salt, glycerol and oxalic acid may include the metal salt and the carbon-based support in a weight ratio of 30:70 to 95:5, 40:60 to 95:5 or 50:50 to 95:5. The weight ratio may be the same as the weight ratio of the metal nanostructure to the carbon-based support in the finally obtained catalyst. In the finally obtained catalyst, the weight ratio of the metal nanostructure to the carbon-based support may be appropriately controlled in consideration of the performance as a catalyst.
[0051] Process for making metal nanostructures and catalysts containing the same
[0052] Figure 1 A schematic reaction scheme illustrating the reaction of an aqueous precursor solution comprising a metal salt, glycerol, oxalic acid, and water.
[0053] Specifically, when part or all of oxalic acid reacts with part of glycerol and is converted into formic acid, part of glycerol may react with part or all of oxalic acid to produce 2-(2,3-dihydroxypropoxy)-2-oxoacetic acid or glycerol monooxalate; 2,3-dihydroxypropyl formate or glycerol monoformate may be produced by a carbon dioxide removal reaction of 2-(2,3-dihydroxypropoxy)-2-oxoacetic acid; and formic acid may be produced by a hydrolysis reaction of 2,3-dihydroxypropyl formate. In this case, glycerol may be regenerated together with formic acid.
[0054] At the same time, despite Figure 1 It is not illustrated in the literature, but the reaction of the aqueous precursor solution including the metal salt, glycerol, oxalic acid and water is carried out in the presence of a carbon-based support.
[0055] Accordingly, the reaction between oxalic acid and glycerol, the reaction between the metal salt and glycerol, and the reaction of loading the metal nanostructure converted from the metal salt on the carbon-based carrier can all be performed in situ.
[0056] The reaction of the aqueous precursor solution including the metal salt, glycerol and oxalic acid in the presence of the carbon-based support may be performed under a heat treatment condition.
[0057] The heat treatment may be performed within a temperature range of 60°C or higher to 110°C or lower, and specifically, within a temperature range of 80°C or higher to 100°C or lower, for 1 hour or more to 24 hours or less, specifically, for 3 hours or more to 10 hours or less, and for example, for 5 hours or more to 8 hours or less.
[0058] The heat treatment can be performed in a non-oxidizing atmosphere, for example, in a reducing atmosphere (hydrogen atmosphere, etc.).
[0059] In the reaction of the precursor aqueous solution including the metal salt, glycerol and oxalic acid in the presence of the carbon-based support, the pH can be maintained in the range of pH 1 or more to pH 9 or less, specifically, in the range of pH 2 or more to pH 5 or less, and for example, in the range of pH 2 or more to pH 3 or less due to formic acid converted from a part of the oxalic acid and the remaining part of the oxalic acid. Here, in order to more accurately control the pH within the desired range, a pH adjuster such as nitrate, sulfate, acetate, NaOH or NH4OH may be further used.
[0060] In the reaction of an aqueous precursor solution including a metal salt, glycerol and oxalic acid in the presence of a carbon-based support, viscosity needs to be controlled.
[0061] The viscosity of the precursor aqueous solution may be in the range of 10 cP or more to 1,000 cP or less, specifically, in the range of 100 cP or more to 500 cP or less, and for example, in the range of 150 cP or more to 300 cP or less.
[0062] For viscosity control, the water content can be set to 50wt% or more to 99wt% or less, specifically, 70wt% or more to 90wt% or less, and for example, 70wt% or more to 80wt% or less based on 100wt% of the precursor aqueous solution.
[0063] Here, the need for viscosity control is as described above.
[0064] (Specific method for producing catalyst)
[0065] Hereinafter, a method of manufacturing a catalyst according to an embodiment will be described in more detail.
[0066] The reaction of an aqueous precursor solution including a metal salt, glycerol and oxalic acid in the presence of a carbon-based carrier may include: a first step of preparing a slurry by dispersing the carbon-based carrier in an aqueous glycerol solution; a second step of reacting the slurry prepared in the first step with an aqueous solution of a metal salt; and a third step of reacting the reaction product of the second step with an aqueous solution of oxalic acid.
[0067] Step 1
[0068] As described above, in the embodiment, in order to reduce the viscosity of glycerin, glycerin is dissolved in water and used in the form of an aqueous solution.
[0069] In this regard, the glycerin aqueous solution of the first step may include glycerin and water in a weight ratio of 10:90 to 50:50, and specifically may include glycerin and water in a weight ratio of 20:80 to 40:60.
[0070] In an embodiment, in order to control the shape and size of the metal nanostructure while uniformly dispersing the carbon-based support in the glycerol aqueous solution, the particle size of the solid in the slurry prepared in the first step may be controlled before adding the slurry to the second step.
[0071] In this regard, before adding the slurry prepared in the first step to the second step, the step of wet grinding or nano-grinding the slurry to prepare a slurry having a solid D90 of less than 10 μm, and specifically, preparing a slurry having a solid D90 of less than 4 μm may be further included.
[0072] Step 2
[0073] The metal salt aqueous solution of the second step may include the metal salt and water in a weight ratio of 30:70 to 70:30, and specifically may include the metal salt and water in a weight ratio of 40:60 to 60:40.
[0074] When the slurry prepared in the first step reacts with the aqueous solution of the metal salt, the weight ratio of the metal salt to the carbon-based support may be set to 50:50 to 80:20.
[0075] The reaction between the slurry prepared in the first step and the aqueous solution of the metal salt may be performed under heat treatment conditions.
[0076] The heat treatment may be performed within a temperature range of 60°C or higher to 110°C or lower, and specifically, within a temperature range of 80°C or higher to 100°C or lower, for 0.1 hour or more to 24 hours or less, specifically, for 3 hours or more to 10 hours or less, and for example, for 5 hours or more to 8 hours or less.
[0077] The heat treatment can be performed in a non-oxidizing atmosphere, for example, in a reducing atmosphere (hydrogen atmosphere, etc.).
[0078] Step 3
[0079] The oxalic acid aqueous solution of the third step may include oxalic acid and water in a weight ratio of 1:1 to 1:10, and specifically, may include oxalic acid and water in a weight ratio of 1:3 to 1:8.
[0080] When the reaction product of the second step is reacted with an aqueous oxalic acid solution, the molar ratio of the metal salt to the oxalic acid may be 1:0.5 to 1:12, specifically, 1:3 to 1:10, more specifically, 1:4 to 1:9, and for example, 1:5 to 1:7. Within such a range, the effects of oxalic acid as a pH adjustment and reduction aid may be improved.
[0081] In the third step, the oxalic acid aqueous solution can be supplied at a rate of 30 ml / min to 70 ml / min, and specifically, the oxalic acid aqueous solution can be supplied at a rate of 40 ml / min to 60 ml / min while being controlled within a temperature range of 50°C to 90°C, and specifically, within a temperature range of 60°C to 80°C, and then mixed with the reaction product of the second step.
[0082] After the supply is completed, the temperature of the mixture of the reaction product of the second step and the aqueous oxalic acid solution is within the range of 90°C to 120°C, and specifically, within the range of 100°C to 110°C, and mixing is performed for 5 to 10 hours while maintaining the temperature range, so that the nucleation and dispersion of the metal nanostructure can be uniform.
[0083] Step 4
[0084] After the third step, a fourth step of aging, filtering, washing and drying may be further included in sequence, which can be regarded as a post-treatment process to increase the purity of the metal nanostructure finally obtained.
[0085] (catalyst)
[0086] In an embodiment, a catalyst including a carbon-based support and a metal nanostructure supported on the carbon-based support is provided, wherein the catalyst inevitably further includes more than 0 ppm to less than 40 ppm of glycerol.
[0087] The catalyst of the embodiment may be a catalyst manufactured by the above method and including an activated metal nanostructure. The activated metal nanostructure strongly adsorbs the material used in the manufacturing process. Accordingly, when the catalyst of the embodiment is analyzed, the material used in the manufacturing process can be detected.
[0088] Residual glycerol
[0089] According to the above method, since glycerol is used as a solvent and a reducing agent, glycerol inevitably remains on the surface of the finally obtained catalyst.
[0090] In the catalyst of the embodiment, the residual amount of glycerol can be measured by the LC-MS method. Specifically, 10 g of the sample is treated with 100 g of water (H2O) and 5 g of ethanol, and then heated at about 90°C for 4 hours. In this process, the glycerol remaining on the surface of the catalyst is released by water and ethanol.
[0091] The released glycerol is measured by LC-MS and HPLC. Here, a dimethylpolysiloxane column as a non-polar column is used, a toluene standard solution with a concentration of 4 g / L is used, and the amount of toluene added is standardized to 4 μg to measure the peak of the organic compound. In the chromatogram obtained above, the area between n-hexane and n-hexadecane is added, and converted into the mass unit of toluene, and the amount of glycerol is calculated. Based on the amount (g) of the sample used in the experiment, the amount (μg) of glycerol is expressed in ppm, ppb or wt%.
[0092] As a result of LC-MS measurement as described above, in the catalyst of the embodiment, the residual amount of glycerol may be greater than 0 ppm and less than 50 ppm, specifically, greater than 0 ppm and less than 40 ppm, and more specifically, 0 ppm or more to 30 ppm or less.
[0093] Residual amount of reactants
[0094] According to the above method, in addition to glycerol, metal salts, oxalic acid, formic acid, etc. are used as reactants. Accordingly, according to the above method, the reactants may inevitably or selectively remain on the surface of the finally obtained catalyst.
[0095] The residual amount of the reactants can also be measured by the LC-MS method. The specific LC-MS measurement method is the same as above, except that "glycerol" is changed to each of the reactants.
[0096] Specifically, in the catalyst of the embodiment, the residual amount of oxalic acid may be 0 ppb or more to less than 20 ppb, specifically, 0 ppb or more to 15 ppb or less, and more specifically, 0 ppb or more to 10 ppb or less.
[0097] In addition, in the catalyst of the embodiment, the residual amount of formic acid may be 0 wt % or more to less than 5 wt %, specifically, 0.1 wt % or more to 3 wt % or less, and more specifically, 0.1 wt % or more to 2 wt % or less.
[0098] Residual amount of pH adjuster
[0099] According to the above method, since a pH regulator such as nitrate, sulfate, acetate, NaOH or NH4OH etc. can be further used, the pH regulator can also be optionally left. The residual amount of the pH regulator can also be measured by the LC-MS method. The specific LC-MS measurement method is the same as above, except that "glycerol" is changed to the pH regulator.
[0100] Residual nitrogen compounds
[0101] In cases where ethylene glycol is used according to the commonly known "polyol" method, when a basic platinum precursor such as (TEA)-2Pt(OH)6, (MEA)-2Pt(OH)6, [Pt(NH3)4]Cl2, [Pt(NH3)4](NO3)2, [Pt(NH3)4](OH)2, Pt(NH3)2Cl2 or (NH4)2[PtCl4] is used, excess nitrogen compounds may inevitably remain on the surface of the ultimately obtained catalyst.
[0102] However, in the case where glycerol is used instead of ethylene glycol according to the above method, the maximum amount of nitrogen compounds remaining in the finally obtained catalyst can be reduced even if a basic platinum precursor is used.
[0103] As a result, in the catalyst of the embodiment, the maximum residual amount of the nitrogen compound may be 0 ppm or more to 50 ppm or less.
[0104] The maximum residual amount of nitrogen compounds can be measured by the N2-TPD method. For example, the maximum residual amount of nitrogen compounds can be determined by the following method: 0.1 g of a sample is charged into a vertical gas flow reactor using quartz wool, 2 L of N2 gas is transferred to the reactor at a heating rate of 10°C / min until the temperature is raised to 400°C, and then the exhaust is measured using a MKS FT-IR analyzer.
[0105] Shape and size of metallic nanostructures
[0106] When ethylene glycol and polyvinyl pyrrolidone are used according to the generally known "polyol" method, it is difficult to uniformly control the shape and size of the metal nanostructures in the finally obtained catalyst to achieve uniform dispersion.
[0107] However, when glycerol and oxalic acid are used according to the above method, the shape and size of the metal nanostructure in the finally obtained catalyst can be uniformly controlled to achieve uniform dispersion. As a result, the metal nanostructure of the embodiment can be spherical metal nanoparticles.
[0108] When the metal nanostructure of the embodiment is subjected to XRD analysis, the grain diameter of the (111) plane may be 0.1 nm or more to 20 nm or less, specifically, 0.5 nm or more to 15 nm or less, and for example, 1 nm or more to 10 nm or less.
[0109] Here, "crystal diameter" refers to the size of crystals connected on the (111) plane of the metal nanostructure, and does not include the particle size of the carbon-based support described below. The crystal diameter can be calculated from the XRD peak half width of the metal nanostructure of the embodiment or the catalyst including the same by the Scherrer equation.
[0110] In addition, when the metal nanostructure of the embodiment is subjected to TEM analysis, the particle size to be observed may be 0.1 nm or more to 20 nm or less, specifically, 0.5 nm or more to 15 nm or less, and for example, may be 1 nm or more to 10 nm or less.
[0111] Weight retention of catalyst during heat treatment
[0112] When glycerol and oxalic acid are used, the weight loss of the finally obtained catalyst can be suppressed.
[0113] When heat-treated at 250° C., the catalyst of the embodiment may have a weight retention rate of 97 wt % to 100 wt %, which is measured according to Equation 1:
[0114] [Equation 1]
[0115] Catalyst weight retention = 100 × (AB) / A
[0116] In equation 1,
[0117] A is the weight of the catalyst before heat treatment, and
[0118] B is the weight of the catalyst after heat treatment.
[0119] (Electrodes, membrane-electrode assemblies, and fuel cell cells for fuel cells)
[0120] The embodiment provides an electrode for a fuel cell cell including the above-mentioned catalyst and an ionomer mixed with the catalyst.
[0121] An embodiment provides a membrane-electrode assembly including an anode and a cathode and an ion exchange membrane between the anode and the cathode, wherein the anode, the cathode, or both correspond to the above-mentioned electrode for a fuel cell cell.
[0122] Embodiments provide a fuel cell unit including a membrane-electrode assembly.
[0123] Since the electrodes, membrane-electrode assemblies, and fuel cell cells are the same as those for general fuel cell cells except that they include the above-mentioned catalyst, a detailed description is omitted.
[0124] [Invention method]
[0125] Hereinafter, specific embodiments of the present invention will be described. However, the embodiments described below are only intended to specifically illustrate or explain the present invention, and are not intended to limit the scope of the present invention.
[0126] Example 1
[0127] (1) Using a high shear dispersing mixer, the carbon-based carrier was dispersed in an aqueous glycerol solution in which glycerol and water (H2O) were mixed at a weight ratio of 50:50. The aqueous glycerol solution in which the carbon-based carrier was dispersed was wet-milled to obtain a slurry having a solid D90 of less than 10 μm.
[0128] (2) A metal salt aqueous solution in which a metal salt and water (H2O) were mixed at a weight ratio of 50:50 was prepared. The metal salt aqueous solution was added to the glycerol slurry in which the carbon-based carrier was dispersed, and then heated to 100° C. for 1 hour. When the metal salt aqueous solution was added, the weight ratio of the metal salt to the carbon-based carrier was set to 60:40.
[0129] (3) An oxalic acid aqueous solution in which oxalic acid and water (H2O) are mixed at a weight ratio of 1:5 is prepared. The oxalic acid aqueous solution is heated to 70°C, and then the heated oxalic acid aqueous solution is pumped into the mixture in which step (2) is completed. Here, the molar ratio of the metal salt to oxalic acid is set to 1:6 in consideration of the size distribution of the final catalyst.
[0130] (4) The final reaction mixture was treated at 100°C for 5 hours, cooled to room temperature, and aged for 12 hours under stirring at 500 rpm. The aged catalyst slurry was filtered and rinsed with hot water to remove water and oxalic acid and its derivatives. The filter cake of the rinsed catalyst reached a final pH of 6.5. The filter cake of the catalyst reaching the above pH was vacuum dried at 100°C, and then further dried at 200°C for 12 hours in a N2-purged oven dryer.
[0131] Example 2
[0132] The catalyst was prepared in the same manner as in Example 1, except that the weight ratio of glycerol to water (H2O) in step (1) was changed to 40:60.
[0133] Example 3
[0134] The catalyst was prepared in the same manner as in Example 1, except that the weight ratio of glycerol to water (H2O) in step (1) was changed to 30:70.
[0135] Example 4
[0136] The catalyst was prepared in the same manner as in Example 1, except that the weight ratio of glycerol to water (H2O) in step (1) was changed to 20:80.
[0137] Example 5
[0138] The catalyst was prepared in the same manner as in Example 1, except that the weight ratio of glycerol to water (H2O) in step (1) was changed to 10:90.
[0139] Example 6
[0140] (1) One or more carbon-based supports are dispersed in a glycerol aqueous solution in which glycerol and water (H2O) are mixed at a weight ratio of 30:70, and then nano-milled to obtain a slurry having a solid D90 of less than 4 μm.
[0141] (2) A metal salt aqueous solution in which a metal salt and water (H2O) were mixed at a weight ratio of 50:50 was prepared. The metal salt aqueous solution was added to the glycerol slurry in which the carbon-based carrier was dispersed, and then heated to 100°C for 1 hour. When the metal salt aqueous solution was added, the weight ratio of the metal salt:carbon-based carrier in the metal salt aqueous solution was set to 60:40.
[0142] (3) An oxalic acid aqueous solution in which oxalic acid and water (H2O) are mixed at a weight ratio of 1:3 is prepared. The oxalic acid aqueous solution is heated to 80°C, and then the heated oxalic acid aqueous solution is pumped into the mixture in which step (2) is completed. Here, considering the size distribution of the final metal nanostructure, the molar ratio of the metal salt to oxalic acid is set to 1:2.
[0143] (4) The final reaction mixture was treated at 100°C for 8 hours, cooled to room temperature, adjusted to pH 2, and aged for 12 hours under stirring at 500 rpm. The aged catalyst slurry was filtered and rinsed with hot water to remove water and oxalic acid and its derivatives. The filter cake of the rinsed catalyst reached a final pH of 6. The filter cake of the catalyst reaching the above pH was vacuum dried at 100°C, and then further dried at 200°C for 12 hours in a N2-purged oven dryer.
[0144] Comparative Example 1
[0145] (1) The carbon-based carrier is dispersed in ethylene glycol using a high shear dispersing mixer. The aqueous ethylene glycol solution in which the carbon-based carrier is dispersed is wet-milled to obtain a solid slurry having a D90 of less than 10 μm.
[0146] (2) A metal salt aqueous solution in which a metal salt and water (H2O) are mixed at a weight ratio of 50:50 is prepared. The metal salt aqueous solution is added to the ethylene glycol slurry in which the carbon-based support is dispersed, and then heated to 100°C for 1 hour. When the metal salt aqueous solution is added, the weight ratio of the metal salt in the metal salt aqueous solution to the carbon-based support in the slurry prepared in step (1) is set to 60:40.
[0147] (3) The final reaction mixture was adjusted to pH 9.5, heated at 180°C for 5 hours, cooled to room temperature, and aged for 12 hours under stirring at 500 rpm. The aged catalyst slurry was filtered and rinsed with hot water to remove water and oxalic acid and its derivatives. The filter cake of the rinsed catalyst reached a final pH of 5. The filter cake of the catalyst reaching the above pH was vacuum dried at 100°C, and then further dried at 200°C for 12 hours in a N2-purged oven dryer.
[0148] [Evaluation Example 1: Evaluation of Catalyst Performance]
[0149] Evaluation Example 1-1: Residual amount of each material remaining on the catalyst surface
[0150] For the catalysts of Examples and Comparative Examples, the residual amount of each material remaining on the catalyst surface was evaluated according to the method described below, and the evaluation results are shown in Table 1.
[0151] (1) Glycerol, oxalic acid and formic acid
[0152] For the catalysts of Examples and Comparative Examples, the residual amount of each of glycerol, oxalic acid, and formic acid was evaluated. The residual amount of each material can be measured by the LC-MS method.
[0153] Specifically, 10 g of the sample was treated with 100 g of water (H2O) and 5 g of ethanol, and then heated at about 90° C. for 4 hours. In this process, glycerol remaining on the surface of the metal nanostructure was released by water and ethanol.
[0154] The released glycerol is measured by LC-MS and HPLC. Here, a dimethylpolysiloxane column as a nonpolar column is used, a toluene standard solution with a concentration of 4 g / L is used, and the amount of toluene added is standardized to 4 μg, to measure the peak of the organic compound. In the chromatogram obtained above, the area between n-hexane and n-hexadecane is added, and converted into the mass unit of toluene, and the amount of glycerol is calculated. Based on the amount (g) of the sample used in the experiment, the amount (μg) of glycerol is expressed in ppm.
[0155] In addition, oxalic acid and formic acid were measured in the same manner as glycerol and expressed in units of ppb and wt%, respectively.
[0156] (2) Nitrogen compounds
[0157] Meanwhile, the catalysts of Examples and Comparative Examples were evaluated for the maximum residual amount of nitrogen compounds.
[0158] The maximum residual amount of nitrogen compounds can be measured by the N2-TPD method. For example, the maximum residual amount of nitrogen compounds can be determined by the following method: 0.1 g of a sample is charged into a vertical gas flow reactor using quartz wool, 2 L of N2 gas is transferred to the reactor at a heating rate of 10°C / min until the temperature rises to 400°C, and then the exhaust is measured using a MKS FT-IR analyzer.
[0159] [Table 1]
[0160] Glycerol (ppm) Oxalic acid (ppb) Formic acid (wt%) Nitrogen compounds (max ppm) Example 1 6 1.3 0.7 22.3 Example 2 9 2.3 0.8 25.4 Example 3 8 1.1 0.8 32.4 Example 4 15 1 0.3 15.2 Example 5 9.3 0.9 0.4 14.6 Example 6 4.3 1.3 0.1 8.4 Comparative Example 1 0 0 0 76
[0161] Evaluation Example 1-2: Crystalline diameter, particle size and weight retention of catalyst
[0162] For the catalysts of Examples and Comparative Examples, the crystallite diameter, particle size, and weight retention were evaluated according to the methods described below, and the evaluation results are shown in Table 2.
[0163] (1) Grain diameter
[0164] For the catalysts of Examples and Comparative Examples, the crystallite diameter of the (111) plane was evaluated by XRD analysis.
[0165] (2) Particle size
[0166] For the catalysts of Examples and Comparative Examples, the particle size was evaluated by TEM analysis.
[0167] (3) Weight retention during heat treatment
[0168] Each of the catalysts of Examples and Comparative Examples was heat-treated at 250° C., and the weight retention rate was evaluated according to Equation 1:
[0169] [Equation 1]
[0170] Weight retention rate = 100 × (AB) / A
[0171] In equation 1,
[0172] A is the weight of the catalyst before heat treatment, and
[0173] B is the weight of the catalyst after heat treatment.
[0174] [Table 2]
[0175]
[0176] Evaluation Example 1-3: Modification and Evaluation of Manufacturing Process
[0177] The catalyst was prepared in the same manner as in Example 1, except that the molar ratio of the metal salt to oxalic acid in the precursor aqueous solution was changed according to Table 3.
[0178] The crystallite diameter of the (111) plane of the catalyst was evaluated in the same manner as in Evaluation Example 2, and the results are shown in Table 3.
[0179] [Table 3]
[0180]
[0181] [Evaluation Example 2: Performance evaluation of catalyst when applied to a fuel cell unit]
[0182] For the catalysts of the examples, the performance of the catalysts when applied to a fuel cell unit was measured, and the results are shown in Table 4.
[0183] (1) Method for manufacturing a fuel cell monomer
[0184] The catalyst loading of the anode is based on Pt of 0.10 mg / cm 2 , and the anode was produced by a printing method. Nafion ionomer (5 wt% Nafion Dispersion, DuPont, USA) was used, and the ratio of ionomer / carbon was 0.9.
[0185] The catalyst loading of the cathode is 0.35 mg / cm based on Pt. 2 , and the cathode was produced by a printing method. Nafion ionomer (5 wt% Nafion Dispersion, DuPont, USA) was used, and the ratio of ionomer / carbon was 0.9.
[0186] The catalyst in each of the anode and the cathode was each of the catalysts of Examples and Comparative Examples.
[0187] As an electrolyte membrane used for producing a membrane-electrode assembly (MEA), NRE211 product (DuPont) was used.
[0188] The anode and the cathode were placed on both sides of the electrolyte membrane, and then pressed at a pressure of 30 bar and 150° C. for 10 minutes to produce a membrane-electrode assembly (MEA).
[0189] (2) Evaluation method of fuel cell monomers
[0190] A single battery cell of 5 cm x 5 cm is connected to a voltmeter and an ammeter. The voltage and current at different points on the IV curve are measured using the voltmeter and the ammeter. The measured values of voltage and current at each point of the IV curve are recorded and plotted on a graph to draw an IV curve with voltage on the y-axis and current on the x-axis. Here, RH100% indicates a relative humidity of 100%.
[0191] Meanwhile, to measure the open circuit voltage (OCV), first, a voltmeter is connected to the fuel cell unit without connecting a load. The voltmeter reads the highest voltage that the cell can generate.
[0192] [Table 4]
[0193]
[0194] result
[0195] According to Tables 1 to 4, in the embodiment represented by the examples, the shape and size of the metal nanostructure are easily controlled under the condition where glycerol and oxalic acid coexist, and the metal nanostructure with the controlled shape and size is supported on a carbon-based support to prepare a catalyst. The process of manufacturing the metal nanostructure and the process of supporting the metal nanostructure on the carbon-based support are performed in situ.
[0196] Since a metal nanostructure having a controlled shape and size is supported on a carbon-based carrier, an embodiment can provide a catalyst having excellent performance and durability. In particular, the catalyst is suitable for use as a catalyst for a fuel cell monomer or a catalyst for water electrolysis.
[0197] While the invention has been described in connection with what are presently considered to be practical embodiments, it should be understood that the invention is not limited to the disclosed embodiments, but, on the contrary, is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the claims.
Claims
1. A method for preparing a catalyst, comprising reacting an aqueous precursor solution comprising a metal salt, glycerol and oxalic acid in the presence of a carbon-based carrier.
2. The method according to claim 1, wherein The precursor aqueous solution including the metal salt, glycerol and oxalic acid includes the metal salt and the carbon-based support in a weight ratio of 30:70 to 95:
5.
3. The method according to claim 1, wherein The molar ratio of the metal salt to the oxalic acid is 1:0.5 to 1:
12.
4. The method according to claim 1, wherein The precursor aqueous solution including the metal salt, glycerol and oxalic acid further includes formic acid.
5. The method according to claim 4, wherein The formic acid is converted from a portion of the oxalic acid.
6. The method according to claim 1, wherein The viscosity of the precursor aqueous solution including the metal salt, glycerol, and oxalic acid is 10 cP or more and 1000 cP or less.
7. The method according to claim 1, wherein The content of water is 50 wt % or more and 99 wt % or less based on 100 wt % of the precursor aqueous solution including the metal salt, glycerol, and oxalic acid.
8. The method according to claim 1, wherein The reaction of the precursor aqueous solution including the metal salt, glycerol, and oxalic acid in the presence of the carbon-based support is performed at a temperature ranging from 60° C. or more to 110° C. or less.
9. The method according to claim 1, wherein The reaction of the precursor aqueous solution including the metal salt, glycerol and oxalic acid in the presence of the carbon-based carrier includes: In the first step, a slurry is prepared by dispersing the carbon-based carrier in a glycerol aqueous solution; The second step is to react the slurry prepared in the first step with an aqueous solution of a metal salt; and In the third step, the reaction product of the second step is reacted with an aqueous oxalic acid solution.
10. The method according to claim 9, wherein In the first step, the glycerol aqueous solution includes glycerol and water in a weight ratio of 10:90 to 50:
50.
11. The method of claim 9, further comprising wet-grinding or nano-grinding the slurry prepared in the first step before adding the slurry to the second step.
12. The method according to claim 9, wherein In the second step, the metal salt aqueous solution includes metal salt and water in a weight ratio of 30:70 to 70:
30.
13. The method according to claim 9, wherein The reaction between the slurry prepared in the first step and the aqueous solution of the metal salt is performed at a temperature ranging from 60° C. to 110° C. for 0.1 hour to 24 hours.
14. The method according to claim 9, wherein In the third step, the oxalic acid aqueous solution includes oxalic acid and water in a weight ratio of 1:1 to 1:
10.
15. The method according to claim 9, wherein In the third step, The oxalic acid aqueous solution is added while the temperature of the oxalic acid aqueous solution is controlled within the range of 50°C to 90°C, and the reaction product of the second step and the oxalic acid aqueous solution are mixed for 5 to 10 hours while the temperature of the mixture of the reaction product of the second step and the oxalic acid aqueous solution is maintained within the range of 90°C to 120°C.
16. The method according to claim 1, further comprising: After the third step, the fourth step of aging, filtering, washing and drying is sequentially performed.
17. A catalyst comprising: Carbon carrier; and The metal nanostructure supported on the carbon carrier, The catalyst inevitably further comprises more than 0 ppm to less than 50 ppm of glycerol.
18. The catalyst according to claim 17, wherein The catalyst inevitably further includes 0 ppb or more and less than 20 ppb of oxalic acid.
19. The catalyst according to claim 17, wherein The catalyst inevitably further includes 0 wt % or more and less than 5 wt % of formic acid.
20. The catalyst according to claim 17, wherein The catalyst has a crystallite diameter of a (111) plane of 0.1 nm or more and 20 nm or less when measured by XRD analysis.
21. The catalyst according to claim 17, wherein The catalyst has a particle size of 0.1 nm or more to 20 nm or less when measured by TEM analysis.
22. The catalyst according to claim 17, wherein When heat treated at 250° C., the catalyst has a weight retention of 97 wt % to 100 wt %, which is calculated according to Equation 1: [Equation 1] Catalyst weight retention = 100 × (AB) / A in, In equation 1, A is the weight of the catalyst before the heat treatment, and B is the weight of the catalyst after the heat treatment.
23. The catalyst according to claim 17, wherein the catalyst is a catalyst for a fuel cell monomer or a catalyst for water electrolysis.