Heat-sensitive recording medium
By using specific color developer and inorganic pigment combinations in the thermally sensitive recording body, combining hollow particles and binder, the problem of insufficient storage and high temperature heat resistance in the existing thermally sensitive recording body is solved, and high sensitivity is achieved and heat-resistant background fogging, improving the overall performance of printing.
Patent Information
- Application Number
- CN202380033793.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-22
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-29
AI Technical Summary
The existing thermal recording bodies have shortcomings in long-term storage and high-temperature heat resistance, especially the heat resistance of 90°C, which cannot meet market demand.
By combining a specific color developer with an inorganic pigment having an oil absorption amount of 130 mL/100 g or less, and using a compound represented by formula (1) as a color developer in the thermally sensitive recording body, combining hollow particles and binder, excellent formation is achieved by using the compound represented by formula (1) as the color developer in the thermally sensitive recording body, the hollow particles and the binder are formed. The basecoat and thermal recording layer enhance the long-term storage and heat-resistant background fogging of printing.
The thermal recording material has achieved excellent performance in long-term printing storage, and has high sensitivity and heat-resistant background fogging resistance, and the plasticizer resistance of the printing part has also been significantly improved.
Smart Images

Figure CN119053452A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thermosensitive recording material. Background Art
[0002] Thermosensitive recording media in widespread practical use record color images by utilizing a heating color development reaction between a colorless or light-colored leuco dye and a phenol or an organic acid. Such thermosensitive recording media have advantages in that, for example, a color image can be formed only by applying heat, and further, a recording device for these can be compact, can be easily maintained, and generates less noise. For this reason, thermosensitive recording media have been used in a wide range of technical fields as various information recording materials for various printing devices such as label printers, automatic ticket machines, CD / ATMs, order output devices used in restaurants, data output devices in scientific research equipment, and the like.
[0003] Generally, developers containing phenolic hydroxyl groups have disadvantages such as poor thermal responsiveness and poor water resistance of the printed portion, and phenolic compounds such as bisphenol A have endocrine problems. Therefore, mainly in Europe, the demand for thermal recording paper containing non-phenolic developers is increasing, and various new non-phenolic developers have been developed.
[0004] For example, Patent Document 1 proposes a thermosensitive recording medium containing 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate as a non-phenolic developer, and reports that the printed portion has excellent water resistance and the background shows high thermal stability. However, although such a developer has excellent resistance to heat background fogging at 90° C., the long-term storage of the print is poor.
[0005] Patent Document 2 reports that a thermosensitive recording medium containing a combination of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and a ureaurethane compound represented by the following formula (2) as a developer has excellent printing running properties.
[0006] However, in Patent Documents 1 and 2, for such developers, only the heat resistance to background fogging up to 90° C. is evaluated. In the market, higher heat resistance is recently required, and heat resistance of 90° C. is insufficient. Therefore, further improvement is required.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent document 1: JP6529197B
[0010] Patent document 2: JP7072130B Summary of the invention
[0011] Problem that the invention aims to solve
[0012] A main object of the present invention is to provide a thermosensitive recording medium which is excellent in long-term preservation of prints.
[0013] A main object of another embodiment of the present invention is to provide a thermosensitive recording medium having high sensitivity and excellent resistance to thermal background fogging and excellent resistance to plasticizers in a printed portion.
[0014] Solutions for solving problems
[0015] The present inventors have conducted extensive studies to achieve the above object and have found that the above object can be achieved by combining a specific developer with an inorganic pigment having an oil absorption of 130 mL / 100 g or less and by combining a compound represented by the following formula (1) with a specific developer. The present invention has been completed based on this finding. More specifically, the present invention provides the following thermosensitive recording material.
[0016] Project 1.
[0017] A thermosensitive recording medium comprising at least an undercoat layer and a thermosensitive recording layer in this order on a support,
[0018] The base coating comprises hollow particles and a binder.
[0019] The heat-sensitive recording layer contains a leuco dye and a developer,
[0020] The thermosensitive recording material contains a compound represented by the following formula (1) as a first developer of the thermosensitive recording layer:
[0021]
[0022] Where R 1 To R 5 are the same or different and each represents a hydrogen atom, a halogen atom, a nitro group, an amino group, an alkyl group, an alkoxy group, an aryloxy group, an alkylcarbonyloxy group, an arylcarbonyloxy group, an alkylcarbonylamino group, an arylcarbonylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a monoalkylamino group, a dialkylamino group or an arylamino group,
[0023] The thermosensitive recording medium meets the following requirements (A) or (B):
[0024] (A) the undercoat layer contains the inorganic pigment I, and the thermosensitive recording layer contains a pigment having an oil absorption of 130 ml / 100 g or less as the inorganic pigment II; or
[0025] (B) The thermosensitive recording layer contains 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureido)phenyl]benzenesulfonamide as the second developer, and contains the second developer in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first developer.
[0026] Project 2.
[0027] The thermosensitive recording material according to item 1, wherein the compound represented by formula (1) is at least one selected from the group consisting of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 2-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and 4-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate.
[0028] Project 3.
[0029] The thermosensitive recording material according to item 1, wherein the compound represented by formula (1) is 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate.
[0030] Project 4.
[0031] The thermosensitive recording material according to any one of items 1 to 3, which satisfies requirement (A).
[0032] Item 5.
[0033] The thermosensitive recording material according to item 4, wherein the content of the inorganic pigment I is 60% by mass or less based on the total solid content of the undercoat layer.
[0034] Item 6.
[0035] The thermosensitive recording material according to item 4 or 5, wherein the oil absorption of the inorganic pigment I is 130 mL / 100 g or less.
[0036] Item 7.
[0037] The thermosensitive recording material according to any one of items 4 to 6, wherein the oil absorption of the inorganic pigment II is 65 mL / 100 g or less.
[0038] Item 8.
[0039] The thermosensitive recording material according to any one of items 4 to 7, wherein the inorganic pigment II is at least one selected from the group consisting of calcium carbonate, aluminum hydroxide and clay.
[0040] Item 9.
[0041] The thermosensitive recording material according to any one of items 1 to 3, which satisfies requirement (B).
[0042] Item 10.
[0043] The thermosensitive recording material according to item 9, wherein the second developer is contained in an amount of 0.9 to 2.5 parts by mass relative to 1 part by mass of the first developer.
[0044] Item 11.
[0045] The thermosensitive recording material according to item 9 or 10, wherein the second developer is 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide.
[0046] Item 12.
[0047] The thermosensitive recording material according to any one of items 9 to 11, wherein the thermosensitive recording layer contains at least one sensitizer selected from the group consisting of dimethyl terephthalate, 1,2-bis(3-methylphenoxy)ethane, stearic acid amide and diphenyl sulfone.
[0048] Item 13.
[0049] The thermosensitive recording material according to any one of items 9 to 11, wherein the thermosensitive recording layer contains at least one sensitizer selected from the group consisting of dimethyl terephthalate and 1,2-bis(3-methylphenoxy)ethane.
[0050] Item 14.
[0051] The thermosensitive recording material according to any one of items 4 to 8, wherein the maximum particle diameter (D100) of the hollow particles is 10 to 30 μm and the average particle diameter (D50) is 3 to 15 μm, the ratio D100 / D50 of the maximum particle diameter (D100) to the average particle diameter (D50) is 1.8 to 3.0, and the volume % of the hollow particles having a particle diameter of 2.0 μm or less is 1% or less.
[0052] Item 15.
[0053] The thermosensitive recording material according to any one of items 9 to 13, wherein the maximum particle diameter (D100) of the hollow particles is 10 to 30 μm and the average particle diameter (D50) is 4.0 to 15 μm, the ratio D100 / D50 of the maximum particle diameter (D100) to the average particle diameter (D50) is 1.8 to 3.0, and the volume % of the hollow particles having a particle diameter of 2.0 μm or less is 1% or less.
[0054] Item 16.
[0055] The thermosensitive recording material according to any one of items 1 to 15, wherein the hollow particles have a hollow ratio of 80% to 98%.
[0056] Item 17.
[0057] The thermosensitive recording material according to any one of items 1 to 16, wherein the content of the hollow particles is 5% by mass to 40% by mass based on the total solid content of the undercoat layer.
[0058] Item 18.
[0059] The thermosensitive recording material according to any one of items 1 to 17, wherein the binder of the undercoat layer comprises a binder resin having a glass transition temperature of -10°C or lower.
[0060] Item 19.
[0061] The thermosensitive recording material according to any one of items 1 to 17, wherein the binder of the undercoat layer comprises a binder resin having a glass transition temperature of -30°C or lower.
[0062] Item 20.
[0063] The thermosensitive recording material according to any one of items 1 to 19, further comprising an adhesive layer on at least one surface of the support.
[0064] Effects of the Invention
[0065] The thermosensitive recording material of the present invention is excellent in long-term storage properties of printed materials.
[0066] A thermosensitive recording medium according to another embodiment of the present invention has high sensitivity and is excellent in resistance to thermal background fogging and excellent in resistance to plasticizers in a printed portion. DETAILED DESCRIPTION
[0067] In the present specification, the expression “includes” or “comprising” includes the following concepts: “comprising,” “consisting essentially of,” and “consisting of.
[0068] In the present specification, a numerical range represented by "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0069] As used herein, "latex" includes latex in the form of a gel or a dry film formed by drying a dispersion medium.
[0070] The present invention relates to a thermosensitive recording medium, which comprises at least an undercoat layer and a thermosensitive recording layer in this order on a support.
[0071] The base coating comprises hollow particles and a binder.
[0072] The heat-sensitive recording layer contains a leuco dye and a developer,
[0073] The thermosensitive recording material contains a compound represented by the following formula (1) as a first developer of the thermosensitive recording layer:
[0074]
[0075] Where R 1 To R 5 are the same or different and each represents a hydrogen atom, a halogen atom, a nitro group, an amino group, an alkyl group, an alkoxy group, an aryloxy group, an alkylcarbonyloxy group, an arylcarbonyloxy group, an alkylcarbonylamino group, an arylcarbonylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a monoalkylamino group, a dialkylamino group or an arylamino group,
[0076] The thermosensitive recording medium meets the following requirements (A) or (B):
[0077] (A) the undercoat layer contains the inorganic pigment I, and the thermosensitive recording layer contains a pigment having an oil absorption of 130 ml / 100 g or less as the inorganic pigment II; or
[0078] (B) The thermosensitive recording layer contains 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureido)phenyl]benzenesulfonamide as the second developer, and contains the second developer in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first developer.
[0079] The thermosensitive recording material having the above-mentioned feature (A) is referred to as "thermosensitive recording material (A)", and the thermosensitive recording material having the above-mentioned feature (B) is referred to as "thermosensitive recording material (B)". They are described in detail below.
[0080] A. Thermosensitive recording medium (A)
[0081] In the present invention, the thermosensitive recording medium comprises at least an undercoat layer and a thermosensitive recording layer in this order on a support.
[0082] The base coating layer comprises hollow particles, a binder and an inorganic pigment I,
[0083] The heat-sensitive recording layer contains a leuco dye, a developer and an inorganic pigment II,
[0084] containing a compound represented by formula (1) (first developer) as a developer,
[0085] A pigment having an oil absorption of 130 ml / 100 g or less is included as the inorganic pigment II.
[0086] Support
[0087] The support in the present invention is not particularly limited in type, shape or size. For example, high-quality paper (acid paper, neutral paper), medium-quality paper, coated paper, coated paper, cast-coated paper, glass paper, resin-laminated paper, polyolefin-based synthetic paper, synthetic fiber paper, non-woven fabric, synthetic resin film, or various transparent supports can be appropriately selected and used. The thickness of the support is not particularly limited, and is generally about 20 to 200 μm. The density of the support is not particularly limited, and is preferably about 0.60 to 0.85 g / cm 3 .
[0088] Base coating
[0089] The thermosensitive recording material of the present invention has an undercoat layer between the support and the thermosensitive recording layer, and the undercoat layer contains hollow particles, a binder, and an inorganic pigment I.
[0090] Hollow particles
[0091] From the viewpoint of enhancing the buffering property, the hollow particles are preferably formed of an organic resin. The undercoat layer containing the hollow particles and thus having excellent heat-insulating properties can prevent the diffusion of heat applied to the thermosensitive recording layer and increase the sensitivity of the thermosensitive recording body.
[0092] Hollow particles formed of organic resins can be divided into foaming type and non-foaming type according to the production method. Of these two types, foaming type hollow particles generally have a larger average particle size and a higher hollow ratio than non-foaming type hollow particles. Therefore, compared with non-foaming type hollow particles, foaming type hollow particles obtain better sensitivity and image quality.
[0093] Non-foamed hollow particles can be produced by polymerizing seeds in a solution, polymerizing other resins to coat the seeds, and removing the seeds inside by swelling and dissolving to form voids inside. The seeds inside are removed by swelling and dissolving using an alkaline aqueous solution or the like. Non-foamed hollow particles having a relatively large average particle size can also be produced by alkali swelling treatment of core-shell particles in which core particles having alkali swelling properties are coated with a shell layer that does not have alkali swelling properties.
[0094] Expandable hollow particles can be produced by preparing particles in which a volatile liquid is sealed in a resin, and causing the liquid in the particles to evaporate and expand while softening the resin by heating.
[0095] In the production process of the foamed hollow particles, the liquid inside the particles is expanded by heating, thereby increasing the hollow ratio and providing excellent heat insulation; therefore, the use of the foamed hollow particles can improve the sensitivity of the thermosensitive recording body and improve the recording concentration. The improvement in sensitivity is particularly important in the color development within the halftone range where the heat energy applied to the thermosensitive recording layer is small. In addition, when the thermosensitive recording layer is formed via an undercoat layer having excellent heat insulation, the diffusion of heat applied to the thermosensitive recording layer is prevented, resulting in excellent image uniformity and improved image quality. Therefore, in this embodiment, it is preferred to use foamed hollow particles that are excellent in improving the heat insulation of the undercoat layer.
[0096] The example of the resin that can be used for foaming type hollow particles includes thermoplastic resin, such as styrene-acrylic resin, polystyrene resin, acrylic resin, polyethylene resin, polypropylene resin, polyacetal resin, chlorinated polyether resin, polyvinyl chloride resin, polyvinylidene chloride resin, acrylic resin (for example, acrylic resin containing acrylonitrile as a component), styrene resin, vinylidene chloride resin and copolymer resin mainly formed by polyvinylidene chloride and acrylonitrile. As the gas contained in the foaming type hollow particles, propane, butane, isobutane, air etc. can be used generally. Among various resins, from the viewpoint of the strength for keeping the shape of the foaming particles, acrylonitrile resin and copolymer resin mainly formed by polyvinylidene chloride and acrylonitrile are preferably used as the resin that can be used for hollow particles.
[0097] The maximum particle size of the hollow particles of the present invention is preferably 10 to 30 μm, and more preferably 10 to 25 μm. The maximum particle size is also referred to as "D100". When the maximum particle size of the hollow particles is 10 μm or more, the cushioning property of the undercoat layer is improved; therefore, the close fit between the thermosensitive recording body and the thermal head during printing is improved, and a thermosensitive recording body with high image quality is obtained. This high image quality can produce an improved recording concentration in a halftone range developed with energy lower than the energy used to provide the maximum recording concentration (Dmax). When the maximum particle size of the hollow particles is 30 μm or less, the smoothness of the undercoat layer is improved; therefore, the thermosensitive recording layer provided via the undercoat layer can be made uniform, and a thermosensitive recording body in which the formation of white spots in the image is less likely to occur can be obtained.
[0098] The average particle size of the hollow particles of the present invention is preferably 3 to 15 μm, and more preferably 5 to 15 μm, or preferably 4.0 to 15 μm, and more preferably 4.5 to 15 μm. The average particle size as used herein is the diameter at which the volume of the larger particle is equal to the volume of the smaller particle when the particles are divided into two types based on the particle size, i.e., the median diameter, which is the particle size corresponding to a frequency of 50 volume %. The average particle size is also referred to as "D50". When the average particle size of the hollow particles is 3 μm or more, the cushioning property of the undercoat layer is improved; therefore, the closeness of the thermosensitive recording body to the thermal head during printing is improved, and a thermosensitive recording body with high image quality is obtained. This high image quality can produce an improved recording concentration in a halftone range developed with energy lower than the energy used to provide the maximum recording concentration (Dmax). When the average particle size of the hollow particles is 15 μm or less, the smoothness of the undercoat layer is improved; therefore, the thermosensitive recording layer provided by the undercoat layer can be made uniform, and a thermosensitive recording body in which white spots are less likely to form in the image can be obtained.
[0099] The maximum particle size (D100) and average particle size (D50) of the hollow particles can be measured using a laser diffraction particle size distribution analyzer. The average particle size (D50) can be shown as the average value of the particle sizes of 10 particles, and the particle size is measured from an image (SEM image) of each particle using an electron microscope.
[0100] The ratio of the maximum particle size (D100) of the hollow particles to the average particle size (D50) of the hollow particles, i.e., D100 / D50, is an index indicating the degree of particle size distribution. The ratio of D100 / D50 is preferably 1.8 to 3.0, and more preferably 2.0 to 2.8. When the ratio of D100 / D50 of the hollow particles is 1.8 or more, the hollow particles can be fully foamed, the maximum particle size will be large enough, the hollow rate will be high, and the heat insulation of the base coating can be improved. When the ratio of D100 / D50 of the hollow particles is 3.0 or less, the size of the hollow particles is uniform, which improves the smoothness of the base coating and suppresses white spots in the image.
[0101] In the particle size distribution measured by a laser diffraction particle size distribution analyzer, the volume % of hollow particles with a particle size of 2.0 μm or less is preferably 1% or less. It is also preferred that the volume % of hollow particles with a particle size of 2.0 μm or less is 0.5%, and more preferably, hollow particles with a particle size of 2.0 μm or less are not included. Hollow particles with a particle size of 2 μm or less are considered to contribute very little to heat insulation because they are too small to have a sufficient hollow area. When the volume % of hollow particles with a particle size of 2 μm or less in the undercoat layer is 1% or less, recording concentration, image quality, etc. can be improved.
[0102] The hollow ratio of the hollow particles is preferably 80% to 98%, and more preferably 90% to 98%. When the hollow ratio of the hollow particles is 80% or more, excellent heat insulation can be imparted to the undercoat layer containing the hollow particles. When the hollow ratio of the hollow particles is 98% or less, the strength of the film around the hollow portion is improved, so that hollow particles that do not collapse even when the undercoat layer is formed can be obtained.
[0103] The hollow ratio of the hollow particles is determined by measuring the true specific gravity according to the IPA method, and the true specific gravity value is used as follows.
[0104] (1) Sample pretreatment
[0105] The samples were dried at 60°C for one day and one night.
[0106] (2) Reagents
[0107] Isopropyl alcohol (IPA: ultrapure reagent)
[0108] (3) Measurement method
[0109] -Weighing volumetric flask (W1).
[0110] - Weigh approximately 0.5 g of the dry sample (W2) in a volumetric flask.
[0111] - Add about 50 mg of IPA thereto, and shake the volumetric flask thoroughly to completely remove the air outside the capsules.
[0112] - Add IPA to the marked line and weigh the volumetric flask (W3).
[0113] - As a blank, add IPA only to the mark on the volumetric flask and weigh the volumetric flask (W4).
[0114] (4) Calculation of true specific gravity
[0115] True specific gravity = {(W2-W1)×((W4-W1) / 100)} / {(W4-W1)-(W3-W2)}
[0116] (5) Calculation of hollow ratio
[0117] Hollowness (%) = {1-1 / (1.1 / true specific gravity)}×100
[0118] The hollow ratio can also be calculated according to the following formula: 3 / D 3 )×100. In the formula, d represents the inner diameter of the hollow particle, and D represents the outer diameter of the hollow particle.
[0119] Since the hollow particles in the present invention have a relatively large particle size, the content of the hollow particles in the undercoat layer can be reduced. The content of the hollow particles is based on the total solid content of the undercoat layer, preferably 5 to 40% by mass, and more preferably 5 to 35% by mass. The hollow particle content of 5% by mass or more can improve the heat insulation of the undercoat layer, and the hollow particle content of 40% by mass or less makes it less likely to cause problems in terms of coating properties, and makes it possible to easily form a uniform undercoat layer and improve the recording concentration. In addition, the coating film strength of the undercoat layer can be improved.
[0120] Binder
[0121] Examples of binders include water-soluble polymer materials, such as polyvinyl alcohol and its derivatives, starch and its derivatives, cellulose derivatives such as hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, methylcellulose and ethylcellulose, sodium polyacrylate, polyvinyl pyrrolidone, acrylamide-acrylate copolymer, acrylamide-acrylate-methacrylate copolymer, styrene-maleic anhydride copolymer, isobutylene-maleic anhydride copolymer, casein, gelatin and its derivatives; emulsions, such as polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylate, vinyl chloride-vinyl acetate copolymer, polybutyl methacrylate and ethylene-vinyl acetate copolymer; and latex of water-insoluble polymers such as styrene-butadiene copolymer and styrene-butadiene-acrylic acid copolymer; etc. Among them, it is preferred to use a binder containing latex. The content of the binder can be selected from a wide range, and based on the total solid content of the primer layer, it is generally preferably about 20% to 70% by mass, and more preferably about 25% to 60% by mass.
[0122] The binder preferably contains a binder resin having a glass transition temperature (Tg) of -10°C or less. When the glass transition temperature is -10°C or less, image quality can be improved even in a low energy range. The glass transition temperature is more preferably -30°C or less because image quality can be further improved in a low energy range. A glass transition temperature of -50°C or less is not preferred because sticking occurs. Therefore, the glass transition temperature is preferably -40°C or more.
[0123] Inorganic Pigments I
[0124] The undercoat layer of the present invention contains an inorganic pigment I. From the viewpoint of increasing the recording density and improving the long-term preservation property, the oil absorption of the inorganic pigment I is preferably 130 mL / 100 g or less, more preferably 125 mL / 100 g or less, and even more preferably 110 mL / 100 g or less. From the viewpoint of effectively reducing printing problems such as the occurrence of head residue and sticking, the oil absorption of the inorganic pigment I is also preferably 40 ml / 100 g or more, more preferably 80 ml / 100 g or more. The oil absorption is a value obtained by the method according to JIS K 5101.
[0125] Various inorganic pigments can be used as the inorganic pigment I, and preferred examples include calcined kaolin and clay, etc. From the viewpoint of improving long-term storage properties, the content of the inorganic pigment I is preferably 60% by mass or less, and more preferably 50% by mass or less based on the total solid content of the undercoat layer. From the viewpoint of effectively reducing printing problems such as the occurrence of head residues and sticking, the content of the inorganic pigment I is also preferably 20% by mass or more, and more preferably 25% by mass or more, based on the total solid content of the undercoat layer.
[0126] For example, the undercoat layer coating liquid is prepared by mixing the hollow particles, the binder, the inorganic pigment I and the auxiliary agent as required using water as a medium, applying the coating liquid to the support, and then drying to form the undercoat layer on the support. The coating amount of the undercoat layer coating liquid is not particularly limited, but is preferably about 2 to 20 g / m2 in terms of dry mass. 2 , more preferably about 2 to 12 g / m 2 .
[0127] Thermal recording layer
[0128] Leuco dye
[0129] The thermosensitive recording layer of the thermosensitive recording medium of the present invention may contain any of various known colorless or light-colored leuco dyes. Specific examples of such leuco dyes are described below.
[0130] Specific examples of the leuco dye include blue color-developing dyes such as 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide, 3-(4-diethylamino-2-methylphenyl)-3-(4-dimethylaminophenyl)-6-dimethylaminophthalide and fluoran; green color-developing dyes such as 3-(N-ethyl-N-p-tolyl)amino-7-N-methylanilinofluoran, 3-diethylamino-7-anilinofluoran, 3-diethylamino-7-dibenzylaminofluoran and rhodamine B-anilinolactam; red color-developing dyes such as 3,6-bis(diethylamino)fluoran-γ-anilinolactam, 3-cyclohexylamino-6-chlorofluoran, 3-diethylamino-6-methyl-7-chlorofluoran, and 3-diethylamino-7-chlorofluoran;Black color-developing dyes, such as 3-(N-ethyl-N-isopentyl)amino-6-methyl-7-anilinofluoran, 3-(N-methyl-N-cyclohexyl)amino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-di(n-butyl)amino-6-methyl-7-anilinofluoran, 3-di(n-pentyl)amino-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isopentylamino)-6-methyl-7-anilinofluoran, 3-diethylamino-7-(m-trifluoromethylanilino)fluoran, 3-(N-isopentyl-N-ethylamino)-7-(o-chloroanilino)fluoran, 3-(N-ethyl-N-2- Tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3-(N-n-hexyl-N-ethylamino)-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-ethylamino]-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-methylamino]-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-methylamino]-6-methyl-7-anilinofluoran, 3-diethylamino-7-(2-chloroanilino)fluoran, 3-di(n-butylamino)-7-(2-chloroanilino)fluoran, 4,4'-bis-dimethylaminobenzodihydroindane benzyl ether, N-2,4,5-trichlorophenylleucoaramine amine), 3-diethylamino-7-butylaminofluoran, 3-ethyl-tolylamino-6-methyl-7-anilinofluoran, 3-cyclohexyl-methylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-chloro-7-(β-ethoxyethyl)aminofluoran, 3-diethylamino-6-chloro-7-(γ-chloropropyl)aminofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-(N-isopentyl-N-ethylamino)-6-methyl-7-anilinofluoran, 3-dibutylamino-7-chloroanilinofluoran, 3-diethylamino-7-(o-chlorophenylamino)fluoran, 3-(N-ethyl-p-toluidinyl)-6-methyl-7-phenyl Aminofluran, 3-(N-ethyl-p-toluidinyl)-6-methyl-7-(p-toluidinyl)fluoran, 3-(N-ethyl-N-tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3-diethylamino-6-chloro-7-anilinofluoran, 3-dimethylamino-6-methyl-7-anilinofluoran, 3-pyrrolidinyl-6-methyl-7-anilinofluoran, 3-piperidinyl-6-methyl-7-anilinofluoran, 2,2-bis{4-[6'-(N-cyclohexyl-N-methylamino)-3'-methylspiro[phthalide-3,9'-xanthone-2'-ylamino]phenyl}propane and 3-diethylamino-7-(3'-trifluoromethylphenyl)aminofluoran;Dyes having an absorption wavelength in the near-infrared region, such as 3,3-bis[1-(4-methoxyphenyl)-1-(4-dimethylaminophenyl)ethylidene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1-(4-methoxyphenyl)-1-(4-pyrrolidinylphenyl)ethylidene-2-yl]-4,5,6,7-tetrachlorophthalide, 3-p-(p-dimethylaminoanilino)anilino-6-methyl-7-chlorofluoran, 3-p-(p-chloroanilino)anilino-6-methyl-7-chlorofluoran, and 3,6-bis(dimethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide; etc. Of course, the usable leuco dyes are not limited to these compounds, and two or more such compounds may be used in combination as required. ;
[0131] The content of the leuco dye is not particularly limited, and is preferably about 3 to 30% by mass, more preferably about 5 to 25% by mass, and even more preferably about 7 to 20% by mass based on the total solid content of the thermosensitive recording layer. A leuco dye content of 3% by mass or more can improve the color developing ability, thereby improving the recording density, while a leuco dye content of 30% by mass or less can improve heat resistance.
[0132] Color developer
[0133] In the present invention, the compound represented by formula (1) is contained as the first color developer. The combination of the compound and the inorganic pigment II can achieve excellent long-term storage properties of prints and the like.
[0134] By R 1 To R 5 The halogen atom represented by may be a fluorine atom, a chlorine atom or a bromine atom, with a fluorine atom and a chlorine atom being preferred.
[0135] The alkyl group may be linear, branched or cyclic, and is preferably a linear or branched alkyl group, and more preferably a linear alkyl group. 1-12 Alkyl, preferably C 1-8 Alkyl, more preferably C 1-6 alkyl, and even more preferably C 1-4 alkyl.
[0136] The alkoxy group may be linear, branched or cyclic, and is preferably a linear or branched alkoxy group, and more preferably a linear alkoxy group. 1-12 Alkoxy, preferably C 2-8 Alkoxy, more preferably C 2-6 Alkoxy, and even more preferably C 2-4 Alkoxy.
[0137] The alkylcarbonyloxy group may be linear, branched or cyclic, and is preferably a linear or branched alkylcarbonyloxy group, and more preferably a linear alkylcarbonyloxy group. The alkylcarbonyloxy group is also preferably C 1-10 Alkylcarbonyloxy.
[0138] The alkylcarbonylamino group may be linear, branched or cyclic, and is preferably a linear or branched alkylcarbonylamino group, and more preferably a linear alkylcarbonylamino group. The alkylcarbonylamino group is also preferably C 1-10 Alkylcarbonylamino.
[0139] The alkylsulfonylamino group may be linear, branched or cyclic, and is preferably a linear or branched alkylsulfonylamino group, and more preferably a linear alkylsulfonylamino group. 1-10 Alkylsulfonylamino.
[0140] The aryl group refers to a monocyclic or polycyclic group formed by one or more 5-membered or 6-membered aromatic hydrocarbon rings. Examples of the aryl group include phenyl, naphthyl and biphenyl.
[0141] The aryloxy group is preferably C 6-12 Aryloxy. Arylcarbonyloxy is preferably C 6-12 Arylcarbonyloxy. Arylcarbonylamino is preferably C 6-12 Arylcarbonylamino. Arylsulfonylamino is preferably C 6-12 Arylsulfonylamino.
[0142] The monoalkylamino group may be linear, branched or cyclic, and is preferably a linear or branched monoalkylamino group, more preferably a linear monoalkylamino group. A monoalkylamino group in which the alkyl group has 1 to 10 carbon atoms is also preferred.
[0143] The dialkylamino group may be linear, branched or cyclic, and is preferably a linear or branched dialkylamino group, and more preferably a linear dialkylamino group. A dialkylamino group in which the alkyl group has 1 to 10 carbon atoms is also preferred.
[0144] The arylamino group may be a monoarylamino group or a diarylamino group, and is preferably C 6-12 Monoarylamino.
[0145] Specific examples of the compound represented by formula (1) include those wherein R 1 To R 5 Each of the compounds is an alkyl group or a hydrogen atom, preferably R 1 To R 5 Each is C 1-8 A compound containing a straight chain alkyl group or a hydrogen atom, more preferably R 1 To R 5 Each is C 1-4A compound containing a straight chain alkyl group or a hydrogen atom, and even more preferably R 1 To R 5 A compound in which each is a methyl group or a hydrogen atom.
[0146] Other specific examples of the compound represented by formula (1) include those wherein R 1 , R 2 , R 4 and R 5 Each is a hydrogen atom and R 3 is a hydrogen atom, a halogen atom, a nitro group, an amino group, an alkyl group, an alkoxy group, an aryloxy group, an alkylcarbonyloxy group, an alkylcarbonylamino group, an arylcarbonylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a monoalkylamino group, a dialkylamino group or an arylamino group (preferably a hydrogen atom or an alkyl group, more preferably a hydrogen atom or a C 1-8 Alkyl, even more preferably a hydrogen atom or a C 1-4 An alkyl group, and a methyl group is particularly preferred.
[0147] The substitution position of the substituent bonded to one benzene ring in the diphenylurea structure in formula (1) may be ortho, meta or para relative to the aminocarbonyl group on the benzene ring, preferably ortho or meta, and more preferably meta.
[0148] The compound represented by formula (1) is not particularly limited, and is preferably at least one selected from the group consisting of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 2-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and 4-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate. Among them, 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate is preferred.
[0149] The content of the compound represented by formula (1) is not particularly limited and can be adjusted according to the leuco dye used. Generally, the content of the compound represented by formula (1) is preferably 0.5 parts by mass or more relative to 1 part by mass of the leuco dye, more preferably 0.8 parts by mass or more, even more preferably 1 part by mass or more, even more preferably 1.2 parts by mass or more, and particularly preferably 1.5 parts by mass or more. The content of the compound represented by formula (1) is also preferably 10 parts by mass or less relative to 1 part by mass of the leuco dye, more preferably 5 parts by mass or less, even more preferably 4 parts by mass or less, and particularly preferably 3.5 parts by mass or less. The content of the compound represented by formula (1) is 0.5 parts by mass or more, which can improve the recording performance. The content of the compound represented by formula (1) is 10 parts by mass or less, which can effectively reduce the background fogging under high temperature environment.
[0150] The thermosensitive recording layer may contain other color developers as long as the effects of the present invention are not impaired.Specific examples of other color developers include phenolic compounds such as 4-tert-butylphenol, 4-acetylphenol, 4-tert-octylphenol, 4,4'-sec-butylidene diphenol, 4-phenylphenol, 4,4'-dihydroxydiphenylmethane, 4,4'-isopropylidene diphenol, 4,4'-cyclohexylidene biphenyl, 4,4'-cyclohexylidene diphenol, 1,1-bis(4-hydroxyphenyl)-ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 4,4'-bis(p-toluenesulfonylaminocarbonylamino)diphenylmethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2'-bis[4-(4-hydroxyphenyl)phenoxy]diethyl ether, 4,4'-dihydroxydiphenyl sulfide, 4,4'-thiobis(3-methylthiophene)sulfide, 4-Hydroxy-6-tert-butylphenol), 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,4'-dihydroxydiphenyl sulfone, 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4-hydroxy-4'-n-propoxydiphenyl sulfone, 4-hydroxy-4'-allyloxydiphenyl sulfone, 4-hydroxy-4'-benzyloxydiphenyl sulfone, 3,3'-diallyl-4,4'-dihydroxydiphenyl sulfone, bis(p-hydroxyphenyl)butyl acetate, bis(p-hydroxyphenyl)methyl acetate, hydroquinone monobenzyl ether, bis(3-allyl-4-hydroxyphenyl) sulfone, 4-hydroxy-4'-methyldiphenyl sulfone, 4-allyloxy-4'-hydroxydiphenyl sulfone, 3,4- dihydroxyphenyl-4'-methylphenyl sulfone, 4-hydroxybenzophenone, dimethyl 4-hydroxyphthalate, methyl 4-hydroxybenzoate, propyl 4-hydroxybenzoate, sec-butyl 4-hydroxybenzoate, phenyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, toluyl 4-hydroxybenzoate, chlorophenyl 4-hydroxybenzoate and 4,4'-dihydroxydiphenyl ether; aromatic carboxylic acids such as benzoic acid, p-chlorobenzoic acid, p-tert-butylbenzoic acid, trichlorobenzoic acid, terephthalic acid, salicylic acid, 3-tert-butylsalicylic acid, 3-isopropylsalicylic acid, 3-benzylsalicylic acid, 3-(α-methylbenzyl)salicylic acid, 3,5-di-tert-butylsalicylic acid, 4-[2-(p-methoxyphenoxy)ethoxy]hydrazine Salicylic acid, 4-[3-(p-toluenesulfonyl)propoxy]salicylic acid, 5-[p-(2-p-methoxyphenoxyethoxy]cumyl]salicylic acid, and zinc 4-[3-(p-toluenesulfonyl)propoxy]salicylate; salts of these phenolic compounds or aromatic carboxylic acids with polyvalent metals such as zinc, magnesium, aluminum, calcium, titanium, manganese, tin and nickel; antipyrine complex of zinc thiocyanate; organic acidic substances such as complex zinc salts of terephthalic acid and other aromatic carboxylic acids; thiourea compounds such as N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenyl urea, N-p-toluenesulfonyl-N'-p-butoxycarbonylphenyl urea, N-p-toluenesulfonyl-N'-phenyl urea and N,N'-di-m-chlorophenylthiourea; having -SO in the molecule. 2NH-bond organic compounds, such as p-cumylphenyl N-(p-toluenesulfonyl)carbamate, p-benzyloxyphenyl N-(p-toluenesulfonyl)carbamate, N-[2-(3-phenylureido)phenyl]benzenesulfonamide and N-(o-toluoyl)-p-toluenesulfonamide; inorganic acidic substances, such as activated clay, attapulgite, colloidal silica and aluminum silicate; etc.
[0151] Examples of other color developers also include ureacarbamate compounds represented by the following formula (2), such as 4,4'-bis[(4-methyl-3-phenoxycarbonylaminophenyl)urea]diphenyl sulfone, 4,4'-bis[(2-methyl-5-phenoxycarbonylaminophenyl)urea]diphenyl sulfone and 4-(2-methyl-3-phenoxycarbonylaminophenyl)urea-4'-(4-methyl-5-phenoxycarbonylaminophenyl)urea diphenyl sulfone; cross-linked diphenyl sulfone compounds represented by the following formula (3); and 4,4'-bis(3-toluenesulfonylurea)diphenylmethane, etc.
[0152]
[0153] Where n=1~6.
[0154] The content of the other developer is not particularly limited, and is preferably 0.5 parts by mass or less, and more preferably 0.3 parts by mass or less, relative to 1 part by mass of the compound represented by formula (1).
[0155] Inorganic Pigments II
[0156] The thermosensitive recording layer of the present invention contains a pigment having an oil absorption of 130 mL / 100 g or less as the inorganic pigment II. The oil absorption of the inorganic pigment II is preferably 125 mL / 100 g or less, more preferably 100 mL / 100 g or less, and most preferably 65 mL / 100 g or less. This significantly improves long-term preservation. From the viewpoint of effectively reducing printing problems such as the occurrence of head residues and adhesion, the oil absorption of the inorganic pigment II is preferably 30 mL / 100 g or more. The thermosensitive recording layer of the present invention may contain a pigment having an oil absorption greater than 130 mL / 100 g, as long as the effect of the present invention is not impaired. Relative to 1 part by mass of the pigment having an oil absorption of 130 mL / 100 g or less, the content of the pigment having an oil absorption greater than 130 mL / 100 g is preferably 0.5 parts by mass or less, more preferably 0.3 parts by mass or less, and even more preferably 0.1 parts by mass or less. It is particularly preferred that the thermosensitive recording layer does not contain a pigment having an oil absorption greater than 130 ml / 100 g. The oil absorption is a value obtained by the method according to JIS K 5101.
[0157] Various inorganic pigments can be used as the inorganic pigment II. Specific examples include inorganic pigments such as calcium carbonate such as light calcium carbonate, aluminum hydroxide, clay such as kaolin, and talc. Among them, the inorganic pigment II is preferably at least one selected from the group consisting of calcium carbonate, aluminum hydroxide and clay. The type of the inorganic pigment II may be different from or the same as the inorganic pigment I. The content of the inorganic pigment II may be selected from a wide range and is preferably 10 to 50% by mass, more preferably 10 to 40% by mass, and even more preferably 15 to 35% by mass based on the total solid content of the thermosensitive recording layer.
[0158] In the present invention, the thermosensitive recording layer may further contain a preservability improver mainly for further enhancing the preservability of the color developed image. As such a preservability improver, for example, a phenol compound selected from 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,1-bis(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisphenol and 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisphenol can be used. At least one of the group consisting of bis(1-methylethylidene)] bisphenol; epoxy compounds such as 4-benzyloxyphenyl-4'-(2-methyl-2,3-epoxypropoxy)phenyl sulfone, 4-(2-methyl-1,2-epoxyethyl)diphenyl sulfone and 4-(2-ethyl-1,2-epoxyethyl)diphenyl sulfone; and isocyanuric acid compounds such as 1,3,5-tris(2,6-dimethylbenzyl-3-hydroxy-4-tert-butyl)isocyanuric acid. Of course, the usable storage improver is not limited to these compounds, and two or more such compounds may be used in combination as needed.
[0159] When a preservability improver is used, its amount used may be an effective amount for improving preservability. The preservability improver is generally preferably used in an amount of about 1 to 25 mass %, and more preferably about 5 to 20 mass %, based on the total solid content of the thermosensitive recording layer.
[0160] In the present invention, the thermosensitive recording layer may further contain a sensitizer. Use of a sensitizer improves recording sensitivity. Examples of usable sensitizers include stearic acid amide, methoxycarbonyl-N-stearic acid benzamide, N-benzoyl stearic acid amide, N-eicosanoic acid amide, ethylene bis stearic acid amide, behenic acid amide, methylene bis stearic acid amide, N-hydroxymethyl stearic acid amide, dibenzyl terephthalate, dimethyl terephthalate, dioctyl terephthalate, diphenyl sulfone, benzyl p-benzyloxybenzoate, 1-hydroxy-2-naphthoic acid phenyl ester, 2-naphthyl benzyl ether, m-terphenyl, p-benzyl biphenyl, oxalic acid-di-p-chlorobenzyl ester, oxalic acid-di-p-methylbenzyl ester, oxalic acid-dibenzyl ester, p-tolyl biphenyl ether, di(p-methoxyphenoxyethyl) ether, 1,2-bis(3-methylphenoxy)ethane, 1,2-bis(4-methylphenoxy)ethane, Ethane, 1,2-bis(4-methoxyphenoxy)ethane, 1,2-bis(4-chlorophenoxy)ethane, 1,2-bisphenoxyethane, 1-(4-methoxyphenoxy)-2-(3-methylphenoxy)ethane, p-methylthiophenylbenzyl ether, 1,4-bis(phenylthio)butane, p-acetyltoluidine, p-acetophenetidide, N-acetoacetyl-p-toluidine, 1,2-bisphenoxytoluene, di(β-biphenylethoxy)benzene, p-bis(vinyloxyethoxy)benzene, 1-isopropylphenyl-2-phenylethane, di-o-chlorobenzyl adipate, 1,2-bis(3,4-dimethylphenyl)ethane, 1,3-bis(2-naphthyloxy)propane, biphenyl, benzophenone, and the like. Among them, 1,2-bis(3-methylphenoxy)ethane is preferred from the viewpoint of obtaining a sensitizing effect without reducing long-term storage properties. These sensitizers can be used in combination as long as the combined use does not impair the effect of the present invention. The content of the sensitizer can be an effective amount for sensitization, and is usually preferably 2 to 25% by mass, more preferably 5 to 20% by mass, and even more preferably 5 to 15% by mass based on the total solid content of the thermosensitive recording layer.
[0161] As other components constituting the thermosensitive recording layer, a binder may be used. In addition, auxiliary agents such as a crosslinking agent, waxes, metal soaps, a water resistance improver, a dispersant, a color dye, and a fluorescent dye may be used as required.
[0162] Examples of the binder include water-soluble polymer materials, such as polyvinyl alcohol and its derivatives, starch and its derivatives, cellulose derivatives such as hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, methylcellulose and ethylcellulose, sodium polyacrylate, polyvinyl pyrrolidone, acrylamide-acrylate copolymer, acrylamide-acrylate-methacrylate copolymer, styrene-maleic anhydride copolymer, isobutylene-maleic anhydride copolymer, casein, gelatin, and its derivatives; emulsions such as polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylate, vinyl chloride-vinyl acetate copolymer, polybutyl methacrylate and ethylene-vinyl acetate copolymer; and latex of water-insoluble polymers such as styrene-butadiene copolymer and styrene-butadiene-acrylic acid copolymer; etc. Among them, polyvinyl alcohol and latex are preferred. The content of the binder can be selected from a wide range, and is generally preferably about 5 to 30% by mass, and more preferably about 10 to 20% by mass based on the total solid content of the thermosensitive recording layer.
[0163] When the thermosensitive recording layer contains a crosslinking agent, the water resistance of the thermosensitive recording layer can be improved. Examples of crosslinking agents include aldehyde compounds such as glyoxal; polyamine compounds such as polyethyleneimine; epoxy compounds, polyamide resins, melamine resins, glyoxylates, dimethylol urea compounds, aziridine compounds, blocked isocyanate compounds; inorganic compounds such as ammonium persulfate, ferric chloride, magnesium chloride, sodium tetraborate and potassium tetraborate; boric acid, boric acid triesters, boron polymers, hydrazide compounds, and glyoxylates, etc. These can be used alone or in combination of two or more. The amount of the crosslinking agent used is preferably about 1 to 5% by mass based on the total solid content of the thermosensitive recording layer.
[0164] The heat-sensitive recording layer is formed on the undercoat layer as follows: for example, by using water as a dispersion medium and using at least one of various agitators or wet pulverizers such as a ball mill, a co-ball mill, a grinder, or a vertical or horizontal sand mill, a leuco dye and a developer, and, if necessary, together with or separately from a sensitizer or a preservability improver, together with a water-soluble synthetic polymer compound such as polyacrylamide, polyvinyl pyrrolidone, polyvinyl alcohol, methylcellulose, or a styrene-maleic anhydride copolymer salt, and other additives such as a surfactant, to form a dispersion; then, the dispersion obtained by reducing the average particle size so that the average particle size is 2 μm or less is mixed with an inorganic pigment II, and optionally further mixed with a binder and an auxiliary agent, etc., to prepare a coating liquid for a heat-sensitive recording layer; the coating liquid for a heat-sensitive recording layer is applied on the undercoat layer; and then dried. The coating amount of the heat-sensitive recording layer is not particularly limited, and is preferably about 1 to 12 g / m in terms of the coating amount after drying. 2 , more preferably 2 to 10 g / m 2 , even more preferably 2.5 to 8 g / m2 , and particularly preferably 3 to 5.5 g / m 2 Note that the thermosensitive recording layer may be formed as two or more separate layers, and the composition and coating amount of each layer may be the same or different, as necessary.
[0165] Protective layer
[0166] As required, the thermosensitive recording medium may include a protective layer formed on the thermosensitive recording layer. The protective layer preferably comprises a pigment and a binder. The protective layer preferably further comprises a lubricant, such as a polyolefin wax or zinc stearate, to prevent the protective layer from adhering to the thermal head. The protective layer may also comprise an ultraviolet light absorber. When a glossy protective layer is formed, the obtained product may have an increased added value.
[0167] The pigment contained in the protective layer is not particularly limited. Examples include inorganic pigments such as amorphous silica, kaolin, clay, light calcium carbonate, heavy calcium carbonate, calcined kaolin, titanium oxide, magnesium carbonate, aluminum hydroxide, colloidal silica, and synthetic layered mica; and plastic pigments such as urea-formalin resin fillers; etc.
[0168] The binder included in the protective layer is not particularly limited, and an aqueous binder selected from a water-soluble binder and a water-dispersible binder can be used. The binder can be appropriately selected from binders that can be used for the heat-sensitive recording layer. Among them, various modified polyvinyl alcohols such as acetoacetyl-modified polyvinyl alcohol, carboxyl-modified polyvinyl alcohol and diacetone-modified polyvinyl alcohol can be more preferably used.
[0169] For example, a protective layer coating liquid is prepared by mixing a pigment and a binder with an auxiliary agent or the like using water as a dispersion medium, applying the coating liquid to the thermosensitive recording layer, and then drying to form a protective layer on the thermosensitive recording layer. The coating amount of the protective layer coating liquid is not particularly limited, and is preferably about 0.3 to 15 g / m in terms of dry mass. 2 , more preferably about 0.3 to 10 g / m 2 , even more preferably about 0.5 to 8 g / m 2 , particularly preferably about 1 to 8 g / m 2 , and more preferably about 1 to 5 g / m 2 The protective layer may be formed as two or more separate layers as necessary, and the composition and coating amount of each layer may be the same or different.
[0170] Other layers
[0171] In the present invention, the thermosensitive recording body preferably has an adhesive layer on at least one surface of the support. This can increase the added value of the thermosensitive recording body. For example, adhesive paper, rewet adhesive paper or delayed adhesive paper can be formed as an adhesive layer by coating one surface of the support with, for example, an adhesive such as an adhesive, a rewet adhesive or a delayed adhesive type adhesive. The recording paper capable of double-sided recording can also be formed by giving the surface of the support opposite to the thermosensitive recording layer as a function of thermal transfer paper, inkjet recording paper, carbonless paper, electrostatic recording paper or electrostatic copy paper. Of course, the thermosensitive recording body can be formed as a double-sided thermosensitive recording body. A back layer can also be provided to suppress the penetration of oil and plasticizer from the back of the thermosensitive recording body, or for curl control and antistatic purposes. The thermosensitive recording body can also be formed as a linerless label that does not require a release paper by forming a release layer containing organic silicon on a protective layer and applying an adhesive to one side.
[0172] Thermal recording medium
[0173] Thermosensitive recording medium can be produced by forming the above-mentioned layers on a support. Any known coating method, such as air knife method, doctor blade method, gravure method, roller coating method, spray coating method, dipping method, rod coating method, curtain coating method, slot die method, slip die method and extrusion method can be used as a method for forming the above-mentioned layers on a support. Each coating liquid can be coated with a first coating liquid and dried, and then coated with a second coating liquid and dried to form layer after layer, or the same coating liquid can be coated separately to form a layer of more than two layers. In addition, simultaneous multi-layer coating can also be carried out, wherein each coating liquid is coated all at once to form a layer of more than two layers at the same time. At any stage after forming each layer or after all layers are formed, the layer can be smoothed by known methods such as super calendering or soft calendering.
[0174] B. Thermosensitive recording medium (B)
[0175] In the present invention, the thermosensitive recording medium comprises at least an undercoat layer and a thermosensitive recording layer in this order on a support.
[0176] The base coating comprises hollow particles and a binder.
[0177] The heat-sensitive recording layer contains a leuco dye, a developer and a binder.
[0178] The thermosensitive recording medium comprises a compound represented by formula (1) as a first developer of the thermosensitive recording layer and 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureido)phenyl]benzenesulfonamide as a second developer of the thermosensitive recording layer,
[0179] The second color developer is contained in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first color developer.
[0180] Support
[0181] The support used in this embodiment may be those described in the section "Support" in the above-mentioned "A. Thermosensitive recording material (A)".
[0182] Base coating
[0183] The thermosensitive recording material of the present invention has an undercoat layer between the support and the thermosensitive recording layer. The undercoat layer contains hollow particles and a binder.
[0184] Hollow particles
[0185] The hollow particles used may be those described in the "Undercoat layer" section in the above "A. Thermosensitive recording material (A)", and the content of the hollow particles may be set as described in the "Undercoat layer" section in the above "A. Thermosensitive recording material (A)".
[0186] Binder
[0187] The binder used may be those described in the "Undercoat layer" section in the above "A. Thermosensitive recording material (A)", and the content of the binder may be set as described in the "Undercoat layer" section in the above "A. Thermosensitive recording material (A)".
[0188] The undercoat layer may contain an oil-absorbing pigment having an oil absorption of 70 ml / 100 g or more, and particularly about 80 to 150 ml / 100 g. The oil absorption is a value determined according to the method of JIS K 5101.
[0189] The oil-absorbing pigment may be any of various types of oil-absorbing pigments. Specific examples include inorganic pigments such as calcined kaolin, amorphous silica, light calcium carbonate and talc. Such oil-absorbing pigments preferably have an average primary particle size of about 0.01 to 5 μm, and particularly about 0.02 to 3 μm. The amount of the oil-absorbing pigment used can be selected from a wide range, and is generally preferably about 20 to 60% by mass, and more preferably about 25 to 55% by mass, based on the total solid content of the undercoat layer.
[0190] For example, the undercoat layer coating liquid is prepared by mixing the hollow particles and the binder and, if necessary, the oil-absorbing pigment and the auxiliary agent using water as a medium, applying the coating liquid to the support, and then drying to form the undercoat layer on the support. The coating amount of the undercoat layer coating liquid is not particularly limited, but is preferably about 2 to 20 g / m2 in terms of dry mass. 2 , and more preferably about 2 to 12 g / m 2 .
[0191] Examples of auxiliary agents that may be included in the coating liquid for the undercoat layer include dispersants such as dioctyl sodium sulfosuccinate, sodium dodecylbenzenesulfonate, sodium lauryl sulfate, and fatty acid metal salts; waxes such as zinc stearate, calcium stearate, polyethylene wax, carnauba wax, paraffin, and ester wax; water-resistant agents such as hydrazide compounds, boric acid, dialdehyde starch, glyoxylates, and epoxy compounds; defoaming agents; coloring dyes; and fluorescent dyes; etc.
[0192] Thermal recording layer
[0193] Leuco dye
[0194] The thermosensitive recording layer of the thermosensitive recording medium of the present invention may contain any of various known colorless or light-colored leuco dyes. The leuco dye used may be those described in the "Thermosensitive recording layer" section in the above "A. Thermosensitive recording medium (A)". The content of the leuco dye may be set as described in the "Thermosensitive recording layer" section in the above "A. Thermosensitive recording medium (A)".
[0195] Color developer
[0196] In the present invention, a first developer and a second developer are contained as developers, and the compound represented by the above-mentioned formula (1) is contained as the first developer.
[0197] The content of the first developer is not particularly limited and can be adjusted according to the leuco dye used. Usually, relative to 1 mass part of leuco dye, the content of the first developer is preferably 0.5 mass parts or more, more preferably 0.8 mass parts or more, even more preferably 1 mass parts or more, even more preferably 1.2 mass parts or more, and particularly preferably 1.5 mass parts or more. Relative to 1 mass part of leuco dye, the content of the first developer is also preferably 10 mass parts or less, more preferably 5 mass parts or less, even more preferably 4 mass parts or less, and particularly preferably 3.5 mass parts or less. A content of 0.5 mass parts or more can improve recording performance. A content of 10 mass parts or less can effectively reduce background fogging under high temperature environments.
[0198] As the second developer, 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureido)phenyl]benzenesulfonamide is included. This allows high sensitivity, excellent resistance to heat background fogging at high temperatures (especially 100°C and 110°C), and resistance to plasticizers. The second developer is preferably 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide.
[0199] The content of the second developer is not particularly limited, and is about 0.4 to 2.5 parts by mass, preferably about 0.7 to 2.5 parts by mass, more preferably about 0.9 to 2.5 parts by mass, and even more preferably about 1.7 to 2.3 parts by mass relative to 1 part by mass of the first developer. A content of the second developer of 0.4 parts by mass or more can improve plasticizer resistance. A content of the second developer of 2.5 parts by mass or less can improve recording performance.
[0200] The thermosensitive recording layer may contain other developers as long as the effects of the present invention are not impaired. Specific examples of other developers include phenolic compounds such as 4-tert-butylphenol, 4-acetylphenol, 4-tert-octylphenol, 4,4'-sec-butylidene diphenol, 4-phenylphenol, 4,4'-dihydroxydiphenylmethane, 4,4'-isopropylidene diphenol, 4,4'-cyclohexylidene biphenyl, 4,4'-cyclohexylidene diphenol, 1,1-bis(4-hydroxyphenyl)-ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 4,4'-bis(p-toluenesulfonylaminocarbonylamino)diphenylmethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2'-bis[4-(4-hydroxyphenyl)phenoxy]diethyl ether, 4,4'-dihydroxydiphenylm ...1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, Phenyl sulfide, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,4'-dihydroxydiphenyl sulfone, 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4-hydroxy-4'-n-propoxydiphenyl sulfone, 4-hydroxy-4'-allyloxydiphenyl sulfone, 4-hydroxy-4'-benzyloxydiphenyl sulfone, 3,3'-diallyl-4,4'-dihydroxydiphenyl sulfone, bis(p-hydroxyphenyl)butyl acetate, bis(p-hydroxyphenyl)methyl acetate, hydroquinone monobenzyl ether, bis(3-allyl-4-hydroxyphenyl) sulfone, 4-hydroxy- 4'-Methyldiphenyl sulfone, 4-allyloxy-4'-hydroxydiphenyl sulfone, 3,4-dihydroxyphenyl-4'-methylphenyl sulfone, 4-hydroxybenzophenone, dimethyl 4-hydroxyphthalate, methyl 4-hydroxybenzoate, propyl 4-hydroxybenzoate, sec-butyl 4-hydroxybenzoate, phenyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, toluyl 4-hydroxybenzoate, chlorophenyl 4-hydroxybenzoate and 4,4'-dihydroxydiphenyl ether; aromatic carboxylic acids such as benzoic acid, p-chlorobenzoic acid, p-tert-butylbenzoic acid, trichlorobenzoic acid, terephthalic acid, salicylic acid, 3-tert-butylsalicylic acid, 3-isopropylsalicylic acid, 3-benzyl salicylic acid Salicylic acid, 3-(α-methylbenzyl)salicylic acid, 3,5-di-tert-butylsalicylic acid, 4-[2-(p-methoxyphenoxy)ethoxy]salicylic acid, 4-[3-(p-toluenesulfonyl)propoxy]salicylic acid, 5-[p-(2-p-methoxyphenoxyethoxy]cumyl]salicylic acid, and zinc 4-[3-(p-toluenesulfonyl)propoxy]salicylate; salts of these phenolic compounds or aromatic carboxylic acids with polyvalent metals such as zinc, magnesium, aluminum, calcium, titanium, manganese, tin and nickel; antipyrine complex of zinc thiocyanate; organic acidic substances such as complex zinc salts of terephthalic acid and other aromatic carboxylic acids; diaryl ureas such as N,N'-di[3-(p-toluenesulfonyl)oxy]phenyl urea;Thiourea compounds, such as N-toluenesulfonyl-N'-3-(toluenesulfonyloxy)phenylurea, N-toluenesulfonyl-N'-butoxycarbonylphenylurea, N-toluenesulfonyl-N'-phenylurea and N,N'-di-m-chlorophenylthiourea; having -SO in the molecule; 2 NH-bond organic compounds, such as p-cumylphenyl N-(p-toluenesulfonyl)carbamate, p-benzyloxyphenyl N-(p-toluenesulfonyl)carbamate and N-(o-toluoyl)-p-toluenesulfonamide; inorganic acidic substances, such as activated clay, attapulgite, colloidal silica and aluminum silicate; etc.
[0201] In the present invention, the thermosensitive recording layer may further contain a preservability improver mainly for further enhancing the preservability of the color developed image. The preservability improver used may be those described in the "Thermosensitive recording layer" section in the above "A. Thermosensitive recording material (A)", and the content of the preservability improver may be set as described in the "Thermosensitive recording layer" section in the above "A. Thermosensitive recording material (A)".
[0202] In the present invention, the thermosensitive recording layer may further contain a sensitizer. Use of a sensitizer improves recording sensitivity. Examples of useful sensitizers include stearic acid amide, methoxycarbonyl-N-stearic acid benzamide, N-benzoyl stearic acid amide, N-eicosanoic acid amide, ethylene bis stearic acid amide, behenic acid amide, methylene bis stearic acid amide, N-hydroxymethyl stearic acid amide, dibenzyl terephthalate, dimethyl terephthalate, dioctyl terephthalate, diphenyl sulfone, benzyl p-benzyloxybenzoate, 1-hydroxy-2-naphthoic acid phenyl ester, 2-naphthyl benzyl ether, m-terphenyl, p-benzyl biphenyl, oxalic acid-di-p-chlorobenzyl ester, oxalic acid-di-p-methylbenzyl ester, oxalic acid-dibenzyl ester, p-tolyl biphenyl ether, di(p-methoxyphenoxyethyl) ether, 1,2-di(3-methylphenoxy)ethane, 1,2-di(4-methylphenoxy)ethane alkane, 1,2-bis(4-methoxyphenoxy)ethane, 1,2-bis(4-chlorophenoxy)ethane, 1,2-diphenoxyethane, 1-(4-methoxyphenoxy)-2-(3-methylphenoxy)ethane, p-methylthiophenyl benzyl ether, 1,4-bis(phenylthio)butane, p-acetyltoluidine, p-acetylethoxyaniline (p-acetophenetidide), N-acetoacetyl-p-toluidine, 1,2-diphenoxytoluene, di(β-biphenylethoxy)benzene, p-di(vinyloxyethoxy)benzene, 1-isopropylphenyl-2-phenylethane, di-o-chlorobenzyl adipate, 1,2-bis(3,4-dimethylphenyl)ethane, 1,3-bis(2-naphthyloxy)propane, biphenyl, and benzophenone, etc. Among them, dimethyl terephthalate, 1,2-bis(3-methylphenoxy)ethane, stearic acid amide and diphenyl sulfone are preferred, and from the viewpoint of obtaining a sensitizing effect without reducing the heat-resistant background fogging at high temperatures, dimethyl terephthalate and 1,2-bis(3-methylphenoxy)ethane are more preferred. These sensitizers may be used in combination as long as the combined use does not impair the effects of the present invention. The content of the sensitizer may be an effective amount for sensitization, and is generally preferably 2 to 25% by mass, more preferably 5 to 20% by mass, and even more preferably 5 to 15% by mass based on the total solid content of the thermosensitive recording layer.
[0203] As other components constituting the thermosensitive recording layer, a binder can be used. In addition, as required, auxiliary agents such as pigments, crosslinking agents, waxes, metal soaps, water resistance improvers, dispersants, colored dyes and fluorescent dyes can be used. The binder and crosslinking agent used can be those described in the "Thermosensitive recording layer" section in the above-mentioned "A. Thermosensitive recording body (A)". The content of the binder and the content of the crosslinking agent can be set as described in the "Thermosensitive recording layer" section in the above-mentioned "A. Thermosensitive recording body (A)".
[0204] The heat-sensitive recording layer is formed on the undercoat layer as follows: for example, by using water as a dispersion medium and using at least one of various agitators or wet pulverizers such as a ball mill, a co-ball mill, a grinder, or a vertical or horizontal sand mill, a leuco dye and a developer, and, if necessary, a sensitizer or a preservability improver together or separately therefrom, together with a water-soluble synthetic polymer compound such as polyacrylamide, polyvinyl pyrrolidone, polyvinyl alcohol, methylcellulose, or a styrene-maleic anhydride copolymer salt, and other additives such as a surfactant, to form a dispersion; then, the dispersion obtained by reducing the average particle size so that the average particle size is 2 μm or less is optionally mixed with a pigment, a binder, an auxiliary agent, etc. to prepare a heat-sensitive recording layer coating liquid; the heat-sensitive recording layer coating liquid is applied to the undercoat layer; and then dried. The coating amount of the heat-sensitive recording layer is not particularly limited, and is preferably about 1 to 12 g / m in terms of the coating amount after drying. 2 , more preferably 2 to 10 g / m 2 , even more preferably 2.5 to 8 g / m 2 , and particularly preferably 3 to 5.5 g / m 2 Note that the thermosensitive recording layer may be formed as two or more separate layers, and the composition and coating amount of each layer may be the same or different, as necessary.
[0205] Protective layer
[0206] The thermosensitive recording material may include a protective layer formed on the thermosensitive recording layer as required. The protective layer used may be those described in the section "Protective layer" in the above-mentioned "A. Thermosensitive recording material (A)".
[0207] Other layers
[0208] In this embodiment, the thermosensitive recording material can be further processed to impart higher functions thereto, thereby increasing added value. The other layers used may be those described in the section "Other layers" in the above-mentioned "A. Thermosensitive recording material (A)".
[0209] Thermal recording medium
[0210] The thermosensitive recording material can be produced by forming the above-mentioned layers on a support. The method for forming each layer may be the method described in the section "Thermosensitive recording material" in the above "A. Thermosensitive recording material (A)".
[0211] Example
[0212] The present invention is described in more detail with reference to examples. However, the present invention is not limited to these examples. In the examples, unless otherwise stated, "parts" and "%" represent "parts by mass" and "% by mass". Particle diameters, such as average particle diameter and maximum particle diameter, are measured using a SALD2200 laser diffraction particle size distribution analyzer (produced by Shimadzu Corporation). "Average particle diameter" used herein refers to median diameter (D50).
[0213] The hollow particles used in Examples and Comparative Examples are as follows.
[0214] Hollow particles A: average particle size (D50): 5.0 μm; maximum particle size (D100): 13.5 μm; hollow ratio: 90%; proportion of particles with a particle size of less than 2 μm: 0.2% by volume; solid content concentration: 15.0%
[0215] Hollow particles B: average particle size (D50): 11 μm; maximum particle size (D100): 23 μm; hollow ratio: 93%; proportion of particles with a particle size of 2 μm or less: 0% by volume; solid content concentration: 15.0%
[0216] Hollow particles C: Ropaque SN-1055 (produced by Dow); average particle size (D50): 1.0 μm; maximum particle size (D100): 1.8 μm; hollow ratio: 55%; solid content concentration: 26.5%
[0217] The average particle size (D50) and the maximum particle size (D100) of these hollow particles were measured at a refractive index of 1.70-0.01i using a SALD2200 laser diffraction particle size analyzer (manufactured by Shimadzu Corporation).
[0218] The latexes used in Examples and Comparative Examples are as follows.
[0219] Latex A: Developed product of styrene-butadiene copolymer latex (Tg: -35°C; particle size: 300nm; solid content concentration: 48%)
[0220] Latex B: Developed product of styrene-butadiene copolymer latex (Tg: -10°C; particle size: 190nm; solid content concentration: 48%)
[0221] Latex C: Styrene-butadiene copolymer latex (trade name: L-1571, produced by Asahi Kasei Corporation; Tg: -3°C; particle size: 190 nm; solid content concentration: 48%)
[0222] The inorganic pigments II used in Examples and Comparative Examples are as follows.
[0223] Calcium carbonate: Trade name: Brilliant-15, produced by Shiraishi Kogyo Kaisha, Ltd.; Oil absorption: 56 ml / 100 g
[0224] Calcium carbonate: Trade name: Cal-Light-KT, produced by Shiraishi Kogyo Kaisha, Ltd.; Oil absorption: 120 ml / 100 g
[0225] Aluminum hydroxide: Trade name: Higilite H-42, produced by Showa Denko KK; Oil absorption: 43 ml / 100 g
[0226] Clay: Trade name: Hydragloss 90, manufactured by KaMin LLC: Oil absorption: 46 ml / 100 g
[0227] Amorphous silica: Trade name: Nipsil E743, manufactured by Tosoh Silica Corporation; Oil absorption: 160 ml / 100 g
[0228] A. Thermosensitive recording medium (A)
[0229] Example A1
[0230] (1) Preparation of coating solution for undercoat layer
[0231] A coating liquid for an undercoat layer is prepared by mixing and stirring 100 parts of hollow particles A, 38 parts of calcined kaolin (trade name: Ansilex 93, produced by BASF; oil absorption: 104 ml / 100 g), 79.2 parts of latex A, 32 parts of a 25% oxidized starch solution, 1.1 parts of carboxymethyl cellulose (trade name: Cellogen AG gum, produced by DKS Co. Ltd.) and 100 parts of water.
[0232] (2) Preparation of leuco dye dispersion (dispersion A1)
[0233] 40 parts of 3-di-(n-butyl)amino-6-methyl-7-anilinofluoran, 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand grinder) to an average particle diameter of 0.5 μm, thereby obtaining a leuco dye dispersion (dispersion A1).
[0234] (3) Preparation of developer dispersion (dispersion B1)
[0235] 40 parts of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid B1).
[0236] (4) Preparation of sensitizer dispersion (dispersion C1)
[0237] 40 parts of 1,2-bis(3-methylphenoxy)ethane (trade name: KS-232, manufactured by Sankosha Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a sensitizer dispersion (dispersion C1).
[0238] (5) Preparation of coating liquid for thermosensitive recording layer
[0239] A coating liquid for a thermosensitive recording layer was prepared by mixing and stirring 29.5 parts of dispersion A1, 63.6 parts of dispersion B1, 45.5 parts of dispersion C1, 70 parts of a 10% aqueous solution of completely saponified polyvinyl alcohol (trade name: PVA117, saponification degree: 99 mol%, average polymerization degree: 1700, produced by Kuraray Co., Ltd.), 20.8 parts of styrene-butadiene copolymer latex (trade name: L-1571, produced by Asahi Kasei Corporation, solid content concentration: 48%), 20 parts of calcium carbonate (trade name: Brilliant-15, produced by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 56 ml / 100 g), 2 parts of adipic acid dihydrazide (produced by Otsuka Chemical Co., Ltd.) and 150 parts of water.
[0240] (6) Preparation of coating liquid for protective layer
[0241] A protective layer coating liquid was prepared by mixing and stirring a composition comprising 317 parts of a 12% aqueous solution of diacetone-modified polyvinyl alcohol (trade name: DF-10, produced by Japan Vam & Poval Co., Ltd.), 60 parts of kaolin (trade name: Hydragloss 90, produced by KaMin LLC), 0.5 parts of polyethylene wax (trade name: Chemipearl W-400, produced by Mitsui Chemicals, Inc., solid content concentration: 40%), 5 parts of zinc stearate (trade name: Hidorin Z-8-36, produced by Chukyo Yushi Co., Ltd., solid content concentration: 36%) and 300 parts of water.
[0242] (7) Production of Thermosensitive Recording Material
[0243] The coating liquid for the undercoat layer, the coating liquid for the thermosensitive recording layer, and the coating liquid for the protective layer were applied in an amount of 4.5 g / m 2 3.8g / m 2 and 2.3 g / m 2 Coated to a basis weight of 60g / m 2 The thermosensitive recording body is obtained by applying a thermosensitive recording layer to the surface of a high-quality paper and drying the film to form an undercoat layer, a thermosensitive recording layer and a protective layer in sequence. The obtained product is then subjected to supercalendering to smooth the surface, thereby obtaining a thermosensitive recording body.
[0244] Example A2
[0245] A thermosensitive recording material was obtained in the same manner as in Example A1 except that aluminum hydroxide (trade name: Higilite H-42, produced by Showa Keikinzoku, oil absorption: 43 ml / 100 g) was used instead of calcium carbonate in the preparation of the thermosensitive recording layer coating liquid in Example A1.
[0246] Example A3
[0247] A thermosensitive recording material was obtained in the same manner as in Example A1 except that clay (trade name: HG90, manufactured by KaMin LLC, oil absorption: 46 ml / 100 g) was used instead of calcium carbonate in the preparation of the thermosensitive recording layer coating liquid of Example A1.
[0248] Example A4
[0249] A thermosensitive recording material was obtained in the same manner as in Example A1, except that calcium carbonate (trade name: Cal-Light-KT, produced by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 120 ml / 100 g) was used instead of calcium carbonate (trade name: Brilliant-15, produced by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 56 ml / 100 g) in the preparation of the coating liquid for the thermosensitive recording layer in Example A1.
[0250] Example A5
[0251] A thermosensitive recording material was obtained in the same manner as in Example A1, except that 79.2 parts of latex B was used instead of 79.2 parts of latex A in the preparation of the undercoat layer coating liquid of Example A1.
[0252] Example A6
[0253] A thermosensitive recording material was obtained in the same manner as in Example A1, except that 79.2 parts of latex C was used instead of 79.2 parts of latex A in the preparation of the undercoat layer coating liquid of Example A1.
[0254] Example A7
[0255] A thermosensitive recording material was obtained in the same manner as in Example A1, except that 100 parts of the hollow particles B were used instead of 100 parts of the hollow particles A in the preparation of the undercoat layer coating liquid of Example A1.
[0256] Example A8
[0257] A thermosensitive recording material was obtained in the same manner as in Example A1, except that in the preparation of the undercoat layer coating liquid of Example A1, the amount of calcined kaolin was changed from 38 parts to 66 parts, the amount of latex A was changed from 79.2 parts to 20.8 parts, and the amount of water was changed from 100 parts to 130 parts.
[0258] Embodiment A9
[0259] A thermosensitive recording material was obtained in the same manner as in Example A1, except that in the preparation of the coating liquid for the undercoat layer of Example A1, the amount of calcined kaolin was changed from 38 parts to 66 parts, 20.8 parts of latex C was used instead of 79.2 parts of latex A, 56.6 parts of hollow particles C were used instead of 100 parts of hollow particles A, and the amount of water was changed from 100 parts to 180 parts.
[0260] Comparative Example A1
[0261] A thermosensitive recording body was obtained in the same manner as in Example A1 except that amorphous silica (trade name: Nipsil E743, produced by Tosoh Silica Corporation) was used instead of calcium carbonate in the preparation of the thermosensitive recording layer coating liquid of Example A1.
[0262] Comparative Example A2
[0263] (8) Preparation of developer dispersion (dispersion D1)
[0264] 40 parts of 4-hydroxy-4'-isopropoxydiphenyl sulfone (trade name: D-8, manufactured by Nippon Soda Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion D1).
[0265] A thermosensitive recording material was obtained in the same manner as in Comparative Example A1, except that in the preparation of the thermosensitive recording layer coating liquid of Comparative Example A1, the developer dispersion liquid D1 was used instead of the developer dispersion liquid B1.
[0266] The Examples and Comparative Examples were evaluated according to the following methods. Table 1 shows the results.
[0267] Record concentration
[0268] An image was recorded on each thermosensitive recording body using a thermosensitive recording evaluation machine (trade name: TH-PMD, produced by Ohkura Electric Co., Ltd.) with an applied energy of 0.13 mJ / dot (halftone color density) and 0.18 mJ / dot (high grayscale color density). The printed portion was measured using a spectrophotometer (X-Rite 504, produced by X-Rite). A larger value indicates a larger print density.
[0269] The evaluation criteria for halftone color density are as follows.
[0270] Color density is above 0.90: Compatible with high-speed printing, very good
[0271] Color density less than 0.90 and 0.80 or more: required for practical use
[0272] Color density less than 0.80: Low sensitivity, has many defects such as white spots, and is problematic in practical use. The evaluation criteria for high grayscale color density are as follows.
[0273] Color density is 1.30 or more: Very good
[0274] Color density less than 1.30 and 1.20 or more: required for practical use
[0275] Color density is less than 1.20: The print density is low, and the long-term preservation of the print is undesirable in actual use.
[0276] An image was recorded on each thermosensitive recording body using a thermosensitive recording evaluation machine (trade name: TH-PMD, produced by Ohkura Electric Co., Ltd.) with applied energy of 0.13 mJ / dot (halftone color density) and 0.18 mJ / dot (high grayscale color density). After each thermosensitive recording body was left to stand in the dark at 23° C. and 50% RH for 3 months, the optical density in the case of halftone color density and in the case of high grayscale color density was measured with a spectrophotometer (X-Rite 504, produced by X-Rite). In addition, the residual rate of the recorded portion was obtained according to the following equation.
[0277] Residual rate (%) = (recording density after treatment / recording density before treatment) × 100
[0278] ·The evaluation criteria are as follows.
[0279] Survival rate 95% or more: Very good
[0280] The residual rate is less than 95% and 85% or more: Good
[0281] Survival rate is less than 85% and 80% or more: No real problem
[0282] The residual rate is less than 80%: the recording density after processing is low, which is problematic in practical use. 90℃ heat resistance
[0283] A sample of each thermosensitive recording medium developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.) was allowed to stand in a chamber at 90° C. for 1 hour. After the treatment, the optical density of the white paper portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite).
[0284] ·The evaluation criteria are as follows.
[0285] The density of the white paper after treatment is 0.10 or less: Very good
[0286] The density of the white paper after treatment is greater than 0.10 and less than 0.20: No problem in actual use
[0287] The density of the processed white paper is greater than 0.20: the background fog is too strong, which is problematic in practical use
[0288] Table 1
[0289]
[0290] As shown in Table 1, the recording density of each thermosensitive recording medium of Examples A1 to A8 is excellent, and there is no practical problem in the long-term preservation of the printing of each thermosensitive recording medium of Examples A1 to A8. Although the halftone density of the thermosensitive recording medium of Example A9 is low, there is no practical problem in the long-term preservation of the printing of the thermosensitive recording medium of Example A9. In contrast, the long-term preservation of the printing of Comparative Example A1 is significantly poor. Comparative Example A2 shows excellent recording density and long-term preservation of the printing by changing the developer; however, the density of the white paper portion is poor in the 90°C heat resistance evaluation.
[0291] B. Thermosensitive recording medium (B)
[0292] Example B1
[0293] (1) Preparation of coating solution for undercoat layer
[0294] A coating liquid for an undercoat layer is obtained by mixing and stirring 56.6 parts of hollow particles C, 70 parts of calcined kaolin (trade name: Ansilex 93, produced by BASF, oil absorption: 105 ml / 100 g), 22.9 parts of latex C, 12 parts of a 25% oxidized starch solution, 6.7 parts of a 15% fully saponified polyvinyl alcohol (trade name: PVA105, saponification degree: 99 mol%, average polymerization degree: 500, produced by Kuraray Co., Ltd.) aqueous solution and 80 parts of water.
[0295] (2) Preparation of leuco dye dispersion (dispersion A2)
[0296] 40 parts of 3-di-(n-butyl)amino-6-methyl-7-anilinofluoran, 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle diameter of 0.5 μm, thereby obtaining a leuco dye dispersion (dispersion A2).
[0297] (3) Preparation of developer dispersion (dispersion B2)
[0298] 40 parts of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid B2).
[0299] (4) Preparation of developer dispersion (dispersion C2)
[0300] 40 parts of 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide, 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, produced by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (produced by Imex Co., Ltd., sand mill) to an average particle size of 1.0 μm, thereby obtaining a developer dispersion (dispersion C2).
[0301] (5) Preparation of sensitizer dispersion (dispersion D2)
[0302] 40 parts of dimethyl terephthalate (produced by Tokyo Chemical Industry Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, produced by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (produced by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a sensitizer dispersion (dispersion D2).
[0303] (6) Preparation of coating liquid for thermosensitive recording layer
[0304] A coating liquid for a thermosensitive recording layer was obtained by mixing and stirring 34.1 parts of dispersion A2, 46.7 parts of dispersion B2, 22.7 parts of dispersion C2, 35 parts of dispersion D2, 63.7 parts of a 15% aqueous solution of completely saponified polyvinyl alcohol (trade name: PVA110, saponification degree: 99 mol%, average polymerization degree: 1000, produced by Kuraray Co., Ltd.), 12.8 parts of latex C (trade name: L-1571, produced by Asahi Kasei Corporation, solid content concentration: 48%), 21 parts of calcium carbonate (trade name: Brilliant-15, produced by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 56 ml / 100 g), 1 part of adipic acid dihydrazide (produced by Otsuka Chemical Co., Ltd.) and 150 parts of water.
[0305] (7) Preparation of coating liquid for protective layer
[0306] A protective layer coating liquid is obtained by mixing and stirring a composition comprising 292 parts of a 12% aqueous solution of acetoacetyl-modified polyvinyl alcohol (trade name: Gohsenx Z-200, produced by Nippon Synthetic Chemical Industry Co., Ltd.), 62 parts of kaolin (trade name: Hydragloss 90, produced by KaMin LLC), 8.3 parts of zinc stearate (trade name: Hidorin Z-9-36, produced by ChukyoYushi Co., Ltd., solid content concentration: 36%) and 150 parts of water.
[0307] (8) Production of Thermosensitive Recording Material
[0308] The coating liquid for the undercoat layer, the coating liquid for the thermosensitive recording layer, and the coating liquid for the protective layer were applied in an amount of 6.5 g / m 2 3.5g / m 2 and 2.3 g / m 2 Coated to a basis weight of 60g / m 2 The thermosensitive recording body is obtained by applying a thermosensitive recording layer to the surface of a high-quality paper and drying the film to form an undercoat layer, a thermosensitive recording layer and a protective layer in sequence. The obtained product is then subjected to supercalendering to smooth the surface, thereby obtaining a thermosensitive recording body.
[0309] Example B2
[0310] A thermosensitive recording material was obtained in the same manner as in Example B1 except that the amount of Dispersion Liquid C2 was changed from 22.7 parts to 34.1 parts and the amount of calcium carbonate was changed from 21 parts to 16 parts in the preparation of the thermosensitive recording layer coating liquid of Example B1.
[0311] Example B3
[0312] A thermosensitive recording material was obtained in the same manner as in Example B1 except that the amount of Dispersion Liquid C2 was changed from 22.7 parts to 45.5 parts and the amount of calcium carbonate was changed from 21 parts to 11 parts in the preparation of the thermosensitive recording layer coating liquid of Example B1.
[0313] Example B4
[0314] A thermosensitive recording material was obtained in the same manner as in Example B1 except that the amount of Dispersion Liquid B2 was changed from 47.7 parts to 22.7 parts and the amount of Dispersion Liquid C2 was changed from 22.7 parts to 47.7 parts in the preparation of the thermosensitive recording layer coating liquid of Example B1.
[0315] Example B5
[0316] (9) Preparation of sensitizer dispersion (dispersion E2)
[0317] 40 parts of 1,2-bis(3-methylphenoxy)ethane (trade name: KS-232, produced by Sankosha Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, produced by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (produced by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a sensitizer dispersion (dispersion E2).
[0318] A thermosensitive recording material was obtained in the same manner as in Example B1, except that in the preparation of the thermosensitive recording layer coating liquid of Example B1, Dispersion Liquid E2 was used instead of Dispersion Liquid D2.
[0319] Example B6
[0320] A thermosensitive recording body was obtained in the same manner as in Example B1, except that in the preparation of the thermosensitive recording layer coating liquid in Example B1, 64 parts of Hymicron L-271 (main component: stearic acid amide, produced by Chukyo Yushi Co., Ltd., solid content concentration: 25%) was used instead of 36.4 parts of dispersion liquid D2.
[0321] Example B7
[0322] (10) Preparation of sensitizer dispersion (dispersion F2)
[0323] 40 parts of diphenyl sulfone (produced by Nicca Chemical Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, produced by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (produced by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a sensitizer dispersion (dispersion F2).
[0324] A thermosensitive recording material was obtained in the same manner as in Example B1, except that in the preparation of the undercoat layer coating liquid of Example B1, Dispersion Liquid F2 was used instead of Dispersion Liquid D2.
[0325] Example B8
[0326] (11) Preparation of developer dispersion (dispersion G2)
[0327] 40 parts of N-[2-(3-phenylureido)phenyl]benzenesulfonamide (trade name: NKK-1304, manufactured by Nippon Soda Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid G2).
[0328] A thermosensitive recording material was obtained in the same manner as in Example B1, except that in the preparation of the thermosensitive recording layer coating liquid of Example B1, Dispersion Liquid G2 was used instead of Dispersion Liquid C2.
[0329] Example B9
[0330] A thermosensitive recording body was obtained in the same manner as in Example B1 except that in the preparation of the thermosensitive recording layer coating liquid of Example B1, the amount of Dispersion Liquid B2 was changed from 47.7 parts to 22.7 parts and 47.7 parts of Dispersion Liquid G2 was used instead of 22.7 parts of Dispersion Liquid C2.
[0331] Example B10
[0332] A thermosensitive recording material was obtained in the same manner as in Example B4, except that in the preparation of the undercoat layer coating liquid of Example B4, 66.7 parts of hollow particles B were used instead of 56.6 parts of hollow particles C, the amount of calcined kaolin (trade name: Ansilex 93, produced by BASF; oil absorption: 105 ml / 100 g) was changed from 70 parts to 30 parts, the amount of latex C was changed from 22.9 parts to 95.8 parts, the amount of 25% oxidized starch solution was changed from 12 parts to 40 parts, and the amount of water was changed from 80 parts to 0 parts.
[0333] Example B11
[0334] A thermosensitive recording material was obtained in the same manner as in Example B10, except that 66.7 parts of the hollow particles A were used instead of 66.7 parts of the hollow particles B in the preparation of the undercoat layer coating liquid of Example B10.
[0335] Example B12
[0336] A thermosensitive recording material was obtained in the same manner as in Example B10, except that 95.8 parts of latex B was used instead of 95.8 parts of latex C in the preparation of the undercoat layer coating liquid of Example B10.
[0337] Example B13
[0338] A thermosensitive recording material was obtained in the same manner as in Example B10, except that 95.8 parts of latex A was used instead of 95.8 parts of latex C in the preparation of the undercoat layer coating liquid of Example B10.
[0339] Comparative Example B1
[0340] (12) Preparation of developer dispersion (dispersion H2)
[0341] 40 parts of 4-hydroxy-4'-isopropoxydiphenyl sulfone (trade name: D-8, manufactured by Nippon Soda Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized to an average particle diameter of 1.0 μm with a sand mill (manufactured by Imex Co., Ltd., sand mill), thereby obtaining a developer dispersion (dispersion H2).
[0342] A thermosensitive recording material was obtained in the same manner as in Example B1, except that in the preparation of the thermosensitive recording layer coating liquid of Example B1, Dispersion Liquid H2 was used instead of Dispersion Liquid B2.
[0343] Comparative Example B2
[0344] (13) Preparation of developer dispersion (dispersion J2)
[0345] 40 parts of N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea (trade name: PF201, manufactured by Solenis), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion J2).
[0346] A thermosensitive recording material was obtained in the same manner as in Example B1, except that in the preparation of the thermosensitive recording layer coating liquid of Example B1, Dispersion Liquid J2 was used instead of Dispersion Liquid B2, the amount of Dispersion Liquid C2 was changed from 22.7 parts to 0 parts, and the amount of calcium carbonate was changed from 21 parts to 31 parts.
[0347] Comparative Example B3
[0348] A thermosensitive recording material was obtained in the same manner as in Example B1, except that in the preparation of the thermosensitive recording layer coating liquid of Example B1, the amount of dispersion liquid B2 was changed from 47.7 parts to 0 parts, the amount of dispersion liquid C2 was changed from 22.7 parts to 44.7 parts, and the amount of calcium carbonate was changed from 21 parts to 31 parts.
[0349] The Examples and Comparative Examples were evaluated according to the following methods. Table 4 shows the results.
[0350] Record concentration
[0351] An image was recorded on each thermosensitive recording medium with an applied energy of 0.18 mJ / dot (halftone color density) using a thermosensitive recording evaluation machine (trade name: TH-PMD, manufactured by Ohkura Electric Co., Ltd.). The printed portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite). A larger value indicates a larger print density.
[0352] The evaluation criteria for halftone color density are as follows.
[0353] Color density is 1.25 or above: compatible with high-speed printing, very good
[0354] Color density is 1.10 or more and less than 1.25: required for practical use
[0355] Color density less than 1.10: Low sensitivity, with many defects such as white spots, which is problematic in practical use
[0356] An image was recorded on each thermosensitive recording medium using a thermosensitive recording evaluation machine (trade name: TH-PMD, produced by Ohkura Electric Co., Ltd.) with an applied energy of 0.25 mJ / dot (highest color density). The printed portion was measured using a spectrophotometer (X-Rite 504, produced by X-Rite). A larger value indicates a larger print density.
[0357] The evaluation criteria for the highest color density are as follows.
[0358] Color density is 1.40 or above: compatible with high-speed printing, very good
[0359] Color density is 1.30 or more and less than 1.40: required for practical use
[0360] Color density less than 1.30: Low sensitivity, with many defects such as white spots, which is problematic in practical use
[0361] Plasticizer resistance
[0362] A wrapping film (trade name: Hi-S Soft, produced by Nippon Carbide Industries Co., Inc.) was wrapped three times around a polycarbonate tube (diameter: 40 mm), and a thermosensitive recording body that had been color-developed using a label printer (trade name: L-2000, produced by Ishida Co., Ltd.) was placed on the film. The wrapping film was further wrapped three times around the thermosensitive recording body, and the wrapped thermosensitive recording body was allowed to stand at 50° C. for 24 hours. After this treatment, the optical density of the recorded portion was measured using a spectrophotometer (X-Rite504, produced by X-Rite), and the residual rate was calculated according to the following: residual rate=(printing density after treatment)÷(printing density before treatment).
[0363] The evaluation criteria for the residual rate are as follows.
[0364] The residual rate after treatment is more than 65%: barcode readable, good
[0365] The residual rate after processing is 40% or more and less than 65%: Visually readable, no practical problem The residual rate after processing is less than 40%: Printing is lost, which is problematic in practical use 100℃ heat resistance
[0366] A sample of each thermosensitive recording medium developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.) was allowed to stand in a chamber at 100° C. for 1 hour. After the treatment, the optical density of the white paper portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite).
[0367] ·The evaluation criteria are as follows.
[0368] Table 2
[0369]
[0370] 110℃ heat resistance
[0371] A sample of each thermosensitive recording medium that had been color-developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.) was allowed to stand in a chamber at 110° C. for 1 hour. After the treatment, the optical density of the white paper portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite).
[0372] ·The evaluation criteria are as follows.
[0373] Table 3
[0374]
[0375] Table 4
[0376]
Claims
1. A thermosensitive recording medium comprising at least an undercoat layer and a thermosensitive recording layer in this order on a support, The base coating layer comprises hollow particles and a binder, The heat-sensitive recording layer contains a leuco dye and a developer, The thermosensitive recording material contains a compound represented by the following formula (1) as a first developer of the thermosensitive recording layer: Where R 1 To R 5 are the same or different and each represents a hydrogen atom, a halogen atom, a nitro group, an amino group, an alkyl group, an alkoxy group, an aryloxy group, an alkylcarbonyloxy group, an arylcarbonyloxy group, an alkylcarbonylamino group, an arylcarbonylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a monoalkylamino group, a dialkylamino group or an arylamino group, The thermosensitive recording medium meets the following requirements (A) or (B): (A) the undercoat layer contains an inorganic pigment I, and the thermosensitive recording layer contains a pigment having an oil absorption of 130 ml / 100 g or less as an inorganic pigment II; or (B) The thermosensitive recording layer contains 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureido)phenyl]benzenesulfonamide as a second developer, and contains the second developer in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first developer.
2. The thermosensitive recording material according to claim 1, wherein the compound represented by the formula (1) is at least one selected from the group consisting of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 2-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and 4-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate.
3. The thermosensitive recording material according to claim 1, which satisfies requirement (A). 4 . The thermosensitive recording material according to claim 3 , wherein the content of the inorganic pigment I is 60% by mass or less based on the total solid content of the undercoat layer. 5 . The thermosensitive recording material according to claim 3 , wherein the oil absorption of the inorganic pigment I is 130 ml / 100 g or less. 6 . The thermosensitive recording material according to claim 3 , wherein the inorganic pigment II is at least one selected from the group consisting of calcium carbonate, aluminum hydroxide and clay.
7. The thermosensitive recording material according to claim 1, which satisfies requirement (B). 8 . The thermosensitive recording material according to claim 7 , wherein the second developer is contained in an amount of 0.9 to 2.5 parts by mass relative to 1 part by mass of the first developer.
9. The thermosensitive recording material according to claim 7, wherein the thermosensitive recording layer contains at least one sensitizer selected from the group consisting of dimethyl terephthalate, 1,2-bis(3-methylphenoxy)ethane, stearic acid amide and diphenyl sulfone.
10. The thermosensitive recording material according to claim 3, wherein the maximum particle size (D100) of the hollow particles is 10 to 30 μm and the average particle size (D50) is 3 to 15 μm, the ratio D100 / D50 of the maximum particle size (D100) to the average particle size (D50) is 1.8 to 3.0, and the volume % of the hollow particles with a particle size of 2.0 μm or less is 1% or less.
11. The thermosensitive recording material according to claim 7, wherein the maximum particle size (D100) of the hollow particles is 10 to 30 μm and the average particle size (D50) is 4.0 to 15 μm, the ratio D100 / D50 of the maximum particle size (D100) to the average particle size (D50) is 1.8 to 3.0, and the volume % of the hollow particles with a particle size of 2.0 μm or less is 1% or less. 12 . The thermosensitive recording material according to claim 1 , wherein the hollow particles have a hollow ratio of 80% to 98%. 13 . The thermosensitive recording material according to claim 1 , wherein the content of the hollow particles is 5% by mass to 40% by mass based on the total solid content of the undercoat layer.
14. The thermosensitive recording material according to any one of claims 1 to 11, wherein the binder of the undercoat layer comprises a binder resin having a glass transition temperature of -10°C or lower.
Citation Information
Patent Citations
Heat-sensitive recording material
JP2021100798A
Thermosensitive recording medium
JP2021171990A
Heat sensitive recording material with non-phenolic color developers
US20210060994A1
Thermosensitive recording body
WO2022050404A1