Fluoropolymer binders for lithium ion secondary battery cathodes

By using a combination of tetrafluoroethylene polymer with high melt creep viscosity and an elastomeric fluoropolymer, the problem of easy rupture of the cathode electrode film of the lithium-ion battery when forming a tubular shape is solved, and the elasticity and stability of the cathode electrode film are achieved , suitable for cathode electrode film of lithium-ion batteries.

CN119054115APending Publication Date: 2024-11-29THE CHEMOURS CO FC LLC +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034950.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-04-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The cathode electrode film of the lithium-ion secondary battery is prone to rupture when forming a tubular shape, resulting in poor performance and it is difficult for the prior art to provide sufficient elasticity and stability.

Method used

Using a fluoropolymer binder composition, including a high melt creep viscosity tetrafluoroethylene polymer and an elastomeric fluoropolymer, dry mixing by solvent-free process and applying shear force to fibrillate tetrafluoroethylene polymer to form a cathode composition with elasticity.

Benefits of technology

This method enables the cathode electrode film of the lithium-ion battery to form a tubular shape without rupture, improves the performance and stability of the battery, and is suitable for the cathode electrode film of the lithium-ion battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054115A_ABST
    Figure CN119054115A_ABST
Patent Text Reader

Abstract

Provided is a fluorine-containing polymer binder composition for a lithium ion secondary battery cathode, the fluorine-containing polymer binder composition containing a tetrafluoroethylene polymer and an elastomeric fluorine-containing polymer. Also provided is a cathode composition containing the fluoropolymer binder composition and cathode active particles and a conductive carbon. The tetrafluoroethylene polymer is generally a tetrafluoroethylene homopolymer and a modified tetrafluoroethylene homopolymer which are high in molecular weight and cannot be melt-molded. The elastomeric fluoropolymer is typically a vinylidene fluoride elastomeric fluoropolymer. The cathode composition is formed by a solvent-free process in a manner of dry mixing the fluoropolymer binder, cathode active material, and conductive carbon and applying a shear force, whereby the tetrafluoroethylene polymer is fibrillated. The cathode composition has a fluoropolymer binder homogeneously dispersed in a main component cathode active material, and has elasticity such that a thin film of the cathode composition can be formed into a cylindrical shape without breaking, thereby enabling them to be used as a lithium ion battery cathode electrode film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fluorine-containing polymer binder composition for a lithium ion secondary battery cathode and a production method thereof. Summary of the invention

[0002] The present invention provides a fluoropolymer binder composition for a lithium ion secondary battery cathode, the fluoropolymer binder composition comprising: i.) tetrafluoroethylene polymer; and ii.) elastomeric fluoropolymer (alternatively referred to herein as fluoroelastomer). The tetrafluoroethylene polymer is generally selected from high molecular weight non-melt-moldable tetrafluoroethylene homopolymers and high molecular weight non-melt-moldable modified tetrafluoroethylene homopolymers. The elastomeric fluoropolymer is generally a vinylidene fluoride elastomeric fluoropolymer. The binder composition is formed by a solvent-free process, generally by dry mixing tetrafluoroethylene polymers and elastomeric fluoropolymers, and in one embodiment, shear forces are applied to the composition, whereby the tetrafluoroethylene polymer is fibrillated.

[0003] The present invention also provides a cathode composition for a lithium ion secondary battery cathode, the cathode composition comprising: the above-mentioned fluorine-containing polymer binder composition, the cathode composition further comprising cathode active particles and conductive carbon. The cathode composition of the present invention has elasticity, so that a calendered film of the composition suitable for use as a cathode electrode film in a lithium ion battery can be formed into a tubular shape without breaking.

[0004] The present invention also provides a method for manufacturing the above-mentioned cathode composition for lithium ion secondary battery cathode, the method comprising: mixing an elastomer fluoropolymer, cathode active particles, tetrafluoroethylene polymer and conductive carbon to form the cathode composition. In one embodiment, the method involves mixing an elastomer fluoropolymer with cathode active particles to form a fluoroelastomer and a cathode active composition, and then mixing the composition with tetrafluoroethylene polymer and conductive carbon to form the cathode composition. The mixing step of the method of the present invention is performed in the absence of solvent, and generally involves dry mixing and applying shear force to the composition of fluoroelastomer, cathode active particles, tetrafluoroethylene polymer and conductive carbon, whereby the shear force is sufficient to fibrillate the tetrafluoroethylene polymer. BRIEF DESCRIPTION OF THE DRAWINGS

[0005] Figure 1 , Figure 2 , Figure 3 and Figure 4 is a graph of the fluorine content distribution obtained by performing LIBS microscopy on a film of the composition of the present invention of a cathode active material, a tetrafluoroethylene polymer and an elastomeric fluoropolymer. DETAILED DESCRIPTION

[0006] In one embodiment, the present invention is a fluoropolymer binder composition for a lithium ion secondary battery cathode, the fluoropolymer binder composition comprising: i.) a tetrafluoroethylene polymer; and ii.) an elastomeric fluoropolymer.

[0007] In another embodiment, the present invention is a cathode composition for a lithium ion secondary battery cathode comprising: i.) a tetrafluoroethylene polymer; ii.) an elastomeric fluoropolymer; iii.) cathode active particles; and iv.) conductive carbon.

[0008] In one embodiment, the cathode composition has elasticity such that a calendered film of the composition suitable for use as a cathode electrode film in a lithium ion battery can be formed into a tubular shape without rupture.

[0009] In one embodiment, the tetrafluoroethylene polymers of the present invention have a 11 In another embodiment, the tetrafluoroethylene polymer has a melt creep viscosity of at least about 2.0×10 11 In another embodiment, the tetrafluoroethylene polymer has a melt creep viscosity of at least about 3.0×10 11 In a preferred embodiment, the tetrafluoroethylene polymer has a melt creep viscosity of at least about 4.0×10 11 In this article, melt creep viscosity (MCV) is measured by the method described in Ebnesajjad, Sina, (2015), Fluoroplastics, Vol. 1 - Non-Melt Processible Fluoropolymers - The Definitive User's Guide and Data Book (2nd Edition), Appendix 5, Melt Creep Viscosity of Polytetrafluoroethylene, pp. 660-661, with reference to U.S. Pat. No. 3,819,594.

[0010] The tetrafluoroethylene polymer of the present invention is a polymer comprising repeating units of tetrafluoroethylene monomer (also known in the art as TFE) and having a carbonyl group of at least about 1.8×10 11In one embodiment, the tetrafluoroethylene polymer is a tetrafluoroethylene homopolymer containing only repeating units of tetrafluoroethylene monomers, also known as polytetrafluoroethylene in the art, abbreviated as PTFE. In another embodiment, the tetrafluoroethylene polymer is a "modified" PTFE, which refers to a copolymer of TFE in which the concentration of the comonomer is so small that the melting point of the resulting polymer will not be significantly reduced to a melting point lower than that of PTFE. The concentration of such comonomers is less than 1% by weight, preferably less than 0.5% by weight. A minimum amount of at least about 0.05% by weight is used to have a significant effect. Example comonomers of modified PTFE include perfluoroolefins, particularly hexafluoropropylene (HFP) or perfluoro(alkyl vinyl ether) (PAVE) in which the alkyl group contains 1 to 5 carbon atoms, preferably perfluoro(ethyl vinyl ether) (PEVE) and perfluoro(propyl vinyl ether) (PPVE). Other examples of comonomers that modify PTFE include chlorotrifluoroethylene (CTFE) and perfluorobutylethylene (PFBE), or other similar comonomers that introduce bulky side groups to the polymer chain.

[0011] In a preferred embodiment, the tetrafluoroethylene polymers of the present invention are fibrillable. By fibrillable is meant that the tetrafluoroethylene polymers are capable of forming nanometer-sized fibrils in at least one dimension (i.e., <100 nm in width), and these fibrils can vary in length from submicrometer to several micrometers when the tetrafluoroethylene polymers are subjected to shear forces, such as during the mixing process of the present invention for making cathode compositions.

[0012] In one embodiment, the elastomeric fluoropolymer of the present invention has a Mooney viscosity of at least about 20 MU measured at condition ML 1+10 (121° C.) according to ASTM D1646. In another embodiment, the elastomeric fluoropolymer of the present invention has a Mooney viscosity of at least about 30 MU measured at condition ML 1+10 (121° C.) according to ASTM D1646. In another embodiment, the elastomeric fluoropolymer of the present invention has a Mooney viscosity of at least about 40 MU measured at condition ML 1+10 (121° C.) according to ASTM D1646. In another embodiment, the elastomeric fluoropolymer of the present invention has a Mooney viscosity of at least about 50 MU measured at condition ML 1+10 (121° C.) according to ASTM D1646. In another embodiment, the elastomeric fluoropolymer of the present invention has a Mooney viscosity of at least about 60 MU measured at condition ML 1+10 (121° C.) according to ASTM D1646. In a preferred embodiment, the elastomeric fluoropolymer of the present invention has a Mooney viscosity of at least about 70 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

[0013] The elastomeric fluoropolymer of the present invention is an elastomer that provides elasticity to the present cathode composition, enabling a calendered film of the composition to be formed into a tubular shape (e.g., a tubular shape having a radius of curvature sufficient for use as a cathode electrode film in a lithium ion battery) without rupture.

[0014] Example elastomeric fluoropolymers include: vinylidene fluoride / hexafluoropropylene (VDF / HFP), vinylidene fluoride / hexafluoropropylene / tetrafluoroethylene (VDF / HFP / TFE), vinylidene fluoride / perfluoro(methyl vinyl ether) / tetrafluoroethylene (VDF / PMVE / TFE), tetrafluoroethylene / perfluoro(methyl vinyl ether) (TFE / PMVE), tetrafluoroethylene / propylene (TFE / P), and ethylene / tetrafluoroethylene / perfluoro(methyl vinyl ether) (E / TFE / PMVE).

[0015] Alternatively, the elastomeric fluoropolymers useful in the present invention may be described as:

[0016] (A) An elastomeric fluoropolymer based on VDF, wherein VDF is copolymerized with at least one additional comonomer selected from the group consisting of:

[0017] (i) C2-C8 perfluoroolefins, such as tetrafluoroethylene (TFE) and hexafluoropropylene (HFP);

[0018] (ii) hydrogen-containing C2-C8 olefins, such as vinyl fluoride (VF), trifluoroethylene, hexafluoroisobutylene, perfluoroalkylethylenes of the formula CH2=CH-Rf (wherein Rf is a C1-C6 perfluoroalkyl group);

[0019] (iii) C2-C8 fluoroolefins containing at least one of iodine, chlorine and bromine, such as chlorotrifluoroethylene (CTFE);

[0020] (iv) (per)fluoroalkyl vinyl ethers (PAVE) of the formula CF2=CFORf, wherein Rf is C1-

[0021] C6 (per)fluoroalkyl group, preferably -CF3, -C2F5, -C3F7;

[0022] (v) (per)fluoro-oxy-alkyl vinyl ethers of the formula CF2=CFOX, wherein X is a C1-C12 ((per)fluoro)-oxyalkyl radical containing a chain oxygen atom, for example a perfluoro-2-propoxypropyl radical;

[0023] (vi) (Per)fluorodioxole;

[0024] (vii) (per)fluoro-methoxy-vinyl ether having the formula: CF2=CFOCF2ORf2, wherein Rf2 is selected from the group consisting of: C1-C6 (per)fluoroalkyl; C5-C6 cyclic (per)fluoroalkyl; and C2-C6 (per)fluorooxyalkyl containing at least one chain oxygen atom;

[0025] Rf2 is preferably -CF2CF3, -CF2CF2OCF3 or -CF3;

[0026] (viii) C2-C8 non-fluorinated olefins, such as ethylene and propylene; and

[0027] (2) An elastomeric fluoropolymer based on TFE, wherein TFE is copolymerized with at least one additional comonomer selected from the group consisting of (i) to (vii) above.

[0028] In a preferred embodiment, the elastomeric fluoropolymer is a copolymer of vinylidene fluoride, more preferably a copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene.

[0029] In one embodiment, the elastomeric fluoropolymer binder is crosslinked. Crosslinking not only improves the mechanical properties of the polymer, but also helps to provide good contact between the components of the cathode composition of the present invention.

[0030] In a preferred embodiment, the fluoropolymer binder composition comprises a melt creep viscosity of at least about 4.0×10 11 The elastomeric fluoropolymer is a tetrafluoroethylene homopolymer having a Mooney viscosity of at least about 17 MU as measured according to ASTM D1646 under Condition ML 1+10 (121° C.).

[0031] In one embodiment, the weight ratio of tetrafluoroethylene polymer to elastomeric fluoropolymer in the binder and cathode composition of the present invention is from about 4:1 to about 1:4. In a preferred embodiment, the weight ratio of tetrafluoroethylene polymer to the elastomeric fluoropolymer is about 1:1. The amount of elastomeric fluoropolymer in the cathode composition can be determined by one of ordinary skill in the art within this range, and is preferably the minimum amount necessary for a film of the cathode composition of the present invention to perform satisfactorily in a cathode having a radius of curvature required for a given lithium ion battery.

[0032] In one embodiment of the cathode composition of the present invention, the amount of fluoropolymer binder is from about 2 wt% to about 10 wt%, the amount of cathode active particles is from about 90 wt% to about 97 wt%, and the amount of conductive carbon is from about 0.1 wt% to about 5 wt%, based on the combined weight of the fluoropolymer binder, cathode active particles and conductive carbon.

[0033] In one embodiment, the amount of tetrafluoroethylene polymer in the cathode composition is about 2 wt%, the amount of elastomeric fluoropolymer is about 2 wt%, the amount of cathode active particles is about 95 wt%, and the amount of conductive carbon is about 1 wt%, based on the combined weight of fluoropolymer binder, cathode active particles, and conductive carbon. In one embodiment, the amount of tetrafluoroethylene polymer in the cathode composition is about 1 wt%, the amount of elastomeric fluoropolymer is about 1 wt%, the amount of cathode active particles is about 97 wt%, and the amount of conductive carbon is about 1 wt%, based on the combined weight of fluoropolymer binder, cathode active particles, and conductive carbon.

[0034] The cathode active particles of the present invention are selected from electrochemical cathode active materials known in the art. Exemplary cathode active particles include metal oxides, metal sulfides or lithium metal oxides. In a preferred embodiment, the cathode active particles comprise lithium transition metal oxides. Exemplary lithium metal oxides include: lithium nickel manganese cobalt oxide (NMC), lithium manganese oxide (LMO), lithium iron phosphate (LiFePO 4 ), lithium cobalt oxide (LCO), lithium titanate (LTO), and / or lithium nickel cobalt aluminum oxide (NCA). In some embodiments, the cathode active material may include, for example, a layered transition metal oxide (such as LiCoO 2 (LCO), Li(NiMnCo)O 2 (NMC), LiNi 0.8 Co 0.15 Al 0.05 O 2 (NCA)), spinel manganese oxides (such as LiMn 2 O 4 (LMO), LiMn1.5 Ni 0.5 O 4 (LMNO)) or olivine (such as LiFePO 4 )、LiNiO 2 、LiNi 1-x Co x O 2 、LiNi 0.85 Co 0.1 Al 0.05 O 2 、LiNi 0.33 Co 0.33 Mn 0.33 O 2 、LiMn 2 O 4 and their combinations.

[0035] The conductive carbon of the present invention is selected from conductive carbon materials known in the art. Exemplary conductive carbon materials that can be used in the present invention include carbon black, porous carbon, carbon nanotubes, carbon fibers, VGCF (vapor grown carbon fibers), graphene sheets, acetylene black, and combinations thereof.

[0036] In one embodiment, the present invention is a method for making a cathode composition for a lithium ion secondary battery cathode comprising: mixing an elastomeric fluoropolymer, cathode active particles, a tetrafluoroethylene polymer, and a conductive carbon to form the cathode composition.

[0037] In one embodiment, the elastomeric fluoropolymer is comminuted at an elevated temperature (e.g., about 80° C. to about 150° C.) sufficient to impart fluidity to the elastomeric fluoropolymer prior to mixing with any other components of the cathode composition. The inventors have discovered that the elastomeric fluoropolymer, which is relatively low in viscosity and in a semi-fluid state, is subsequently mixed with the cathode active particles, conductive carbon, and tetrafluoroethylene polymer, resulting in a substantially uniform dispersion of all components of the cathode composition. Without wishing to be bound by theory, the inventors believe that when forming the cathode composition of the present invention, the elastomeric fluoropolymer, in a semi-fluid or fluid state, acts as a viscous lubricant that is compatible with the tetrafluoroethylene polymer, thereby improving the mixing of the cathode composition components (shown in the present experimental results by a shorter mixer torque peak time) and improving the dispersion of the cathode composition components (shown in the present experimental results by improved laser induced breakdown spectroscopy (LIBS) results).

[0038] In one embodiment, the present invention is a method for making a cathode composition for a lithium ion secondary battery cathode, the method comprising: i.) mixing an elastomeric fluoropolymer with cathode active particles to form a fluoroelastomer and a cathode active composition, and ii.) mixing the fluoroelastomer and the cathode active composition with a tetrafluoroethylene polymer to form a cathode composition. In one embodiment of the method, the starting form of the elastomeric fluoropolymer is a pellet or a sheet. In one embodiment, prior to step i.) mixing the elastomeric fluoropolymer with the cathode active material, the elastomeric fluoropolymer pellets or sheets are crushed at an elevated temperature (e.g., about 80°C to about 150°C) sufficient to impart fluidity to the elastomeric fluoropolymer, resulting in the pellets or sheets being combined into a uniform continuous semi-fluid body of the elastomeric fluoropolymer, which results in the elastomeric fluoropolymer being better mixed and substantially uniformly dispersed throughout the cathode active material.

[0039] In an alternative embodiment, in the mixing step i.), the fluoroelastomer and cathode active composition is a concentrate containing from about 1 wt.% to about 5 wt.% fluoroelastomer and from about 90 wt.% to about 97 wt.% cathode active particles, and then in the mixing step ii.) the additional elastomeric fluoropolymer is added.

[0040] In a preferred embodiment, the mixing step is performed in the absence of a solvent. In other words, the mixing step is performed by dry blending, wherein the components of the cathode composition are in dry form, such as agglomerates, granules, beads, pellets, flakes or powders.

[0041] In one embodiment, the mixing step ii.) is performed by applying shear forces to the composition of fluoroelastomer, cathode active particles, tetrafluoroethylene polymer and conductive carbon, whereby the shear forces are sufficient to fibrillate the tetrafluoroethylene polymer.

[0042] In one embodiment, the temperature of the mixing step is from about 80°C to about 150°C. In another embodiment, the temperature of the mixing step is about 120°C.

[0043] In one embodiment, the mixing step is performed in a mixer wherein the fill factor is from about 75% to about 95% and the maximum mixing torque occurs within about 0.5 minutes to about 3 minutes of starting mixing. Mixers useful in the process of the present invention can be readily determined by one of ordinary skill in the art and include mixers capable of generating high shear forces and generally suitable for uniformly mixing plastic and rubber materials.

[0044] In the method of the present invention, the dispersion degree of the tetrafluoroethylene polymer and the fluoroelastomer in the cathode composition produced by the mixing step can be determined by laser induced breakdown spectroscopy (LIBS). The dispersion degree of the tetrafluoroethylene polymer and the fluoroelastomer in the cathode composition is ideally high enough to make the cathode composition suitable for use as a cathode electrode film in a lithium ion battery.

[0045] In a preferred embodiment, the tetrafluoroethylene polymer and the fluoroelastomer are dispersed in the cathode composition to an extent that results in a cathode composition that is sufficiently elastic so that a calendered film of the cathode composition can be formed into a tubular shape without failure, such as cracking, splitting, crazing, or other structural discontinuities that may result in poor cathode performance.

[0046] Example

[0047] Material

[0048] a. Cathode active material: LMO (lithium manganese oxide) dry powder, supplier is Posco Es Materials

[0049] b.PTFE1(P1): tetrafluoroethylene homopolymer dry powder, melt creep viscosity is 4.0×10 11 The supplier is Chemours FC LLC

[0050] c.PTFE2(P2): modified tetrafluoroethylene dry powder, melt creep viscosity is 1.8×10 11 The supplier is Chemours FC LLC

[0051] d.PTFE3(P3): modified tetrafluoroethylene dry powder, melt creep viscosity is 1.3×10 10 The supplier is Chemours FC LLC

[0052] e. Fluoroelastomer 1 (F1): VDF / HFP copolymer pellets or sheets, Mooney viscosity of 65MU measured under condition ML 1+10 (100°C) according to ASTM D1646, supplier is Chemours FC LLC

[0053] f. Fluoroelastomer 2 (F2): VDF / HFP / TFE copolymer pellets or sheets, Mooney viscosity of 75MU measured under condition ML1+10 (121°C) according to ASTM D1646, supplier: Chemours FC LLC

[0054] g. Fluoroelastomer 3 (F3): VDF / TFE / PMVE copolymer pellets or sheets, with a Mooney viscosity of 65MU measured under condition ML1+10 (121°C) according to ASTM D1646, and the supplier is Chemours FC LLC

[0055] h. Fluoroelastomer 4 (F4): VDF / HFP / TFE copolymer pellets or sheets, with a Mooney viscosity of 23MU measured under condition ML1+10 (121°C) according to ASTM D1646, and the supplier is Chemours FC LLC

[0056] process

[0057] A certain amount of elastomeric fluoropolymer (rubbery / elastic pellets or sheets) is added to a Brabender mixer and pulverized at 60 RPM for 1 minute at 120°C to produce an elastomeric fluoropolymer with lower viscosity and a semi-fluid continuum. A certain amount of cathode active particles is then added to the Brabender mixer to mix with the semi-fluid elastomeric fluoropolymer and evenly distribute the elastomeric fluoropolymer throughout the cathode active particle matrix. Mixing is performed at 60 RPM for 0.5 minutes at 120°C. A certain amount of tetrafluoroethylene polymer binder powder is then added to the Brabender mixer and mixed with the previously formed cathode active particles and elastomeric fluoropolymer mixture to evenly distribute the tetrafluoroethylene polymer binder powder throughout the cathode active particle matrix and fibrillate the tetrafluoroethylene polymer. Mixing was performed at 120°C and 60 RPM for a period of time sufficient to observe MPT (maximum time to peak torque (minutes)) and MPTQ (maximum peak torque (kgf.m)), i.e., evidence of fibrillation of the tetrafluoroethylene polymer, and then mixing was continued under these conditions for an additional 5 minutes. The cathode mixture formed was then removed from the mixer, cooled to room temperature and observed visually (by the naked eye) and by SEM (scanning electron microscope) to assess the degree of mixing and the dispersion of the elastomeric fluoropolymer and the tetrafluoroethylene polymer throughout the cathode active particle continuous phase, and to assess the degree of fibrillation of the tetrafluoroethylene polymer. A portion of the cathode mixture so formed was removed and pressed at a temperature of 120°C to 200°C to form a 200 micron thick film. The resulting film was then observed visually (by the naked eye), by SEM (scanning electron microscope) and by laser induced breakdown spectroscopy (LIBS) microscopy.

[0058] To enable analysis of the dispersion of cathode composition components by SEM and LIBS, conductive carbon was excluded from these example compositions because conductive carbon is complex and would hinder sample analysis by SEM and / or LIBS. However, when included in the cathode composition, conductive carbon did not substantially change the observed experimental mixing, dispersion, and fibrillation results.

[0059] result

[0060] Table 1 Symbols: Ex = Example number; C = cathode active material (wt%); P1 = PTFE1 (wt%); P2 = PTFE2 (wt%); P3 = PTFE3 (wt%); F1 = fluoroelastomer 1 (wt%); F2 = fluoroelastomer 2 (wt%); F3 = fluoroelastomer 3 (wt%); F1 = fluoroelastomer 4 (wt%); FF = mixer filling factor (mixer volume %); MPT = peak torque maximum time (min); MPTQ = maximum peak torque (kgf.m); ST = mixer set temperature (°C); CT = mixer chamber measurement temperature (°C)

[0061] Table 1

[0062]

[0063] In all examples shown in Table 1, the RPM (revolutions per minute) of the mixer was set to 60 RPM.

[0064] Example 11 is a composition of the following: 97 wt% cathode active material (LMO), 2 wt% PTFE1 (P1) (tetrafluoroethylene homopolymer dry powder, relatively high melt creep viscosity: 4.0×10 11 poise) and 1 wt % of fluoroelastomer 2 ((F2) (VDF / HFP / TFE copolymer, relatively high Mooney viscosity: 75 MU measured according to ASTM D1646 at condition ML 1+10 (121° C.). The mixer filling factor was 95%, the mixer peak torque maximum time was 0.5 minutes, the mixer maximum peak torque was 15.6 kgf.m, the mixer set temperature was 150° C., and the mixer chamber measured temperature was 139.2° C. Figure 1 is a graph of the fluorine content distribution obtained from LIBS microscopy performed on a film of the composition of Example 11. The graph shows that the fluoropolymer binder component of the composition is effectively and uniformly dispersed throughout the main component cathode active material. The 200 micron thick film of the composition of Example 11 was found to have sufficient elasticity to enable the film to be formed into a tubular shape without breaking, and therefore has utility as a cathode electrode film in a lithium ion battery.

[0065] Example 12 is the same as Example 11 except that the mixer fill factor is 85%, the mixer peak torque maximum time is 1 minute, the mixer maximum peak torque is 15.4 kgf.m, the mixer set temperature is 120°C, and the mixer chamber measured temperature is 112.9°C. Figure 2 is a graph of the fluorine content distribution obtained from LIBS microscopy performed on a film of the composition of Example 12. The graph shows that the fluoropolymer binder component of the composition is very effectively and uniformly dispersed throughout the main component cathode active material. The 200 micron thick film of the composition of Example 12 was found to have sufficient elasticity to enable the film to be formed into a tubular shape without breaking, and therefore has utility as a cathode electrode film in a lithium ion battery.

[0066] Example 1 is a comparative composition of the following without the elastomeric fluoropolymer: 97 wt% cathode active material (LMO) and 3 wt% PTFE1 (P1) (tetrafluoroethylene homopolymer dry powder, relatively high melt creep viscosity: 4.0×10 11 The mixer filling factor was 85%, the mixer peak torque maximum time was 3 minutes, the mixer maximum peak torque was 23.5 kgf.m, the mixer set temperature was 150°C, and the mixer chamber measured temperature was 143.0°C. Figure 3 is a graph of the fluorine content distribution obtained from LIBS microscopy performed on a film of the composition of Example 1. The graph shows that in the absence of an elastomeric fluoropolymer, the fluoropolymer binder component of the composition is not effectively dispersed in the cathode active material, the main component in the dry mixing process of the present invention. It was found that the 200 micron thick film of the composition of Example 1 had insufficient elasticity to allow the film to be formed into a tubular shape without breaking, and therefore was unlikely to be used as a cathode electrode film in a lithium ion battery.

[0067] Example 13 is a comparative composition of the following: 97 wt% cathode active material (LMO) and 2 wt% PTFE1 (P1) (tetrafluoroethylene homopolymer dry powder, relatively high melt creep viscosity: 4.0×10 11 poise) and 1 wt% of fluoroelastomer 4 ((F4): VDF / HFP / TFE copolymer pellets or sheets, relatively high Mooney viscosity: 23MU measured according to ASTM D1646 at condition ML 1+10 (121°C). The mixer filling factor is 85%, the mixer peak torque maximum time is 1.5 minutes, the mixer maximum peak torque is 12.4 kgf.m, the mixer set temperature is 120°C, and the mixer chamber measured temperature is 116.1°C. Figure 4is a graph of the fluorine content distribution obtained from LIBS microscopy performed on the film of the composition of Example 13. The graph shows that by using an elastomeric fluoropolymer having a relatively low Mooney viscosity, the fluoropolymer binder component of the composition is not effectively dispersed in the cathode active material, the main component in the dry mixing process of the present invention. It was found that the 200 micron thick film of the composition of Example 13 had insufficient elasticity, making it impossible for the film to be formed into a tubular shape without breaking, and therefore it is unlikely to be used as a cathode electrode film in a lithium ion battery.

Claims

1. A fluoropolymer binder composition for a lithium ion secondary battery cathode, the fluoropolymer binder composition comprising: i.) a tetrafluoroethylene polymer; and ii.) an elastomeric fluoropolymer.

2. The adhesive composition according to claim 1, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

3. The adhesive composition according to claim 1, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

4. The adhesive composition according to claim 1, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

5. The adhesive composition according to claim 1, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

6. The binder composition of claim 1, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 20 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

7. The binder composition of claim 1, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 30 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

8. The binder composition of claim 1, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 40 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

9. The binder composition of claim 1, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 50 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

10. The binder composition of claim 1, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 60 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

11. The binder composition of claim 1, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 70 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

12. The binder composition of claim 1, wherein the elastomeric fluoropolymer is a vinylidene fluoride elastomeric fluoropolymer.

13. The adhesive composition of claim 1, wherein the vinylidene fluoride elastomeric fluoropolymer comprises a copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene.

14. The binder composition according to claim 1, wherein the tetrafluoroethylene polymer is a tetrafluoroethylene homopolymer.

15. The adhesive composition according to claim 1, wherein the tetrafluoroethylene polymer is selected from the group consisting of a high molecular weight non-melt-formable tetrafluoroethylene homopolymer and a high molecular weight non-melt-formable modified tetrafluoroethylene homopolymer.

16. The adhesive composition according to claim 1, wherein the tetrafluoroethylene polymer has a carbon content of at least about 4.0×10 11 The elastomeric fluoropolymer is a tetrafluoroethylene homopolymer having a melt creep viscosity of at least about 150 MU as measured according to ASTM D1646 under condition ML 1+10 (121° C.), and the elastomeric fluoropolymer is a copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene having a Mooney viscosity of at least about 17 MU as measured according to ASTM D1646 under condition ML 1+10 (121° C.).

17. The binder composition of claim 1, wherein the weight ratio of the tetrafluoroethylene polymer to the elastomeric fluoropolymer is from about 4:1 to about 1:

4.

18. The binder composition of claim 1, wherein the tetrafluoroethylene polymer is fibrillated.

19. The adhesive composition of claim 1, formed by a solvent-free process.

20. The binder composition of claim 1, wherein the composition is formed by dry blending the tetrafluoroethylene polymer and the elastomeric fluoropolymer.

21. The binder composition of claim 1, wherein the composition is formed by dry blending the tetrafluoroethylene polymer and the elastomeric fluoropolymer and applying a shear force to the composition, whereby the tetrafluoroethylene polymer is fibrillated.

22. A cathode composition for a lithium ion secondary battery cathode, the cathode composition comprising: i.) a fluoropolymer binder comprising a mixture of a tetrafluoroethylene polymer and an elastomeric fluoropolymer; ii.) cathode active particles; and iii.) conductive carbon; the cathode composition has elasticity so that a calendered film of the composition suitable for use as a cathode electrode film in a lithium ion battery can be formed into a tubular shape without breaking.

23. The cathode composition of claim 22, wherein the cathode active particles comprise a lithium transition metal oxide.

24. The adhesive composition according to claim 1, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

25. The cathode composition of claim 22, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

26. The cathode composition of claim 22, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

27. The cathode composition of claim 22, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

28. The cathode composition of claim 22, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 20 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

29. The cathode composition of claim 22, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 30 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

30. The cathode composition of claim 22, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 40 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

31. The cathode composition of claim 22, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 50 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

32. The cathode composition of claim 22, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 60 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

33. The cathode composition of claim 22, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 70 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

34. The cathode composition of claim 22 wherein the elastomeric fluoropolymer is a vinylidene fluoride elastomeric fluoropolymer.

35. The cathode composition of claim 22, wherein the vinylidene fluoride elastomeric fluoropolymer comprises a copolymer of vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene.

36. The cathode composition of claim 22, wherein the tetrafluoroethylene polymer is a tetrafluoroethylene homopolymer.

37. The cathode composition of claim 22, wherein the tetrafluoroethylene polymer is selected from the group consisting of a high molecular weight non-melt-formable tetrafluoroethylene homopolymer and a high molecular weight non-melt-formable modified tetrafluoroethylene homopolymer.

38. The cathode composition of claim 22, wherein the tetrafluoroethylene polymer is a polymer having a carbon content of at least about 4.0×10 11 The elastomeric fluoropolymer is a tetrafluoroethylene homopolymer having a melt creep viscosity of at least about 150 MU as measured according to ASTM D1646 under condition ML 1+10 (121° C.), and the elastomeric fluoropolymer is a copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene having a Mooney viscosity of at least about 17 MU as measured according to ASTM D1646 under condition ML 1+10 (121° C.).

39. A cathode composition according to claim 22, wherein the amount of the fluoropolymer binder in the cathode composition is from about 5 wt% to about 10 wt%, the amount of the cathode active particles is from about 90 wt% to about 97 wt%, and the amount of the conductive carbon is from about 0.1 wt% to about 1 wt%, based on the combined weight of the fluoropolymer binder, the cathode active particles and the conductive carbon.

40. A cathode composition according to claim 22, wherein the amount of tetrafluoroethylene polymer is about 2 weight percent, the amount of elastomeric fluoropolymer is about 1 weight percent, the amount of cathode active particles is about 96 weight percent, and the amount of conductive carbon is about 1 weight percent, based on the combined weight of the fluoropolymer binder, the cathode active particles, and the conductive carbon.

41. The cathode composition of claim 22, wherein the tetrafluoroethylene polymer is fibrillated.

42. The cathode composition of claim 22, formed by a solvent-free process.

43. The cathode composition of claim 22, wherein the composition is formed by dry blending the tetrafluoroethylene polymer, the elastomeric fluoropolymer, the cathode active particles, and the conductive carbon.

44. The cathode composition of claim 22, wherein the composition is formed by dry blending the tetrafluoroethylene polymer, the elastomeric fluoropolymer, the cathode active particles, and the conductive carbon and applying shear forces to the composition, whereby the tetrafluoroethylene polymer is fibrillated.

45. A method for making a cathode composition for a lithium ion secondary battery cathode, the method comprising: An elastomeric fluoropolymer, cathode active particles, tetrafluoroethylene polymer, and conductive carbon are mixed to form the cathode composition.

46. ​​The method of claim 45 wherein prior to said mixing, said elastomeric fluoropolymer is comminuted at an elevated temperature sufficient to impart flow properties to said elastomeric fluoropolymer.

47. The method of claim 46, wherein the elevated temperature is from about 80°C to about 150°C.

48. The method of claim 45, comprising: i.) mixing the elastomeric fluoropolymer with the cathode active particles to form a fluoroelastomer and cathode active composition; and ii.) mixing the fluoroelastomer and cathode active composition with a tetrafluoroethylene polymer and conductive carbon; to form the cathode composition.

49. The method of claim 48 wherein prior to said step i.) mixing, said elastomeric fluoropolymer is comminuted at an elevated temperature sufficient to impart flow properties to said elastomeric fluoropolymer.

50. The method of claim 49, wherein the elevated temperature is from about 80°C to about 150°C.

51. The method of claim 48 wherein the step i.) fluoroelastomer and cathode active composition is a concentrate containing from about 1 wt.% to about 5 wt.% fluoroelastomer and from about 90 wt.% to about 97 wt.% cathode active material and wherein in step ii.) additional elastomeric fluoropolymer is added.

52. The method of claim 45, wherein the cathode composition comprises from about 1 wt% to about 5 wt% tetrafluoroethylene polymer, from about 1 wt% to about 5 wt% elastomeric fluoropolymer, from about 90 wt% to about 97 wt% cathode active material, and from about 0.1 wt% to about 1 wt% conductive carbon.

53. The method of claim 45 wherein the weight ratio of the tetrafluoroethylene polymer to the elastomeric fluoropolymer is from about 4:1 to about 1:

4.

54. The method of claim 45, wherein the mixing is performed in the absence of a solvent.

55. The method of claim 45, wherein the mixing is performed by dry mixing.

56. The method of claim 45 wherein said mixing is performed by applying shear forces to said combination of fluoroelastomer, cathode active particles, tetrafluoroethylene polymer, and conductive carbon, whereby said shear forces are sufficient to fibrillate said tetrafluoroethylene polymer.

57. The method of claim 45, wherein the mixing is performed at a temperature of about 80°C to about 150°C.

58. The method of claim 45, wherein the mixing is performed at a temperature of about 120°C.

59. The method of claim 45, wherein the mixing is performed in a mixer with a fill factor of about 75% to about 95% and a maximum mixing torque occurring within about 0.5 minutes to about 3 minutes of initiating mixing.

60. The method of claim 45, wherein the degree of dispersion of the tetrafluoroethylene polymer and the fluoroelastomer in the cathode composition as determined by laser induced breakdown spectroscopy (LIBS) is sufficiently high to render the cathode composition suitable for use as a cathode electrode film in a lithium ion battery.

61. The method of claim 45, wherein the cathode composition has elasticity such that a calendered film of the composition can be formed into a tubular shape without rupture.

62. The method of claim 45, wherein the cathode active particles comprise a lithium transition metal oxide.

63. The method of claim 45, wherein the tetrafluoroethylene polymer has a molecular weight of at least about 1.8 x 10 11 Melt creep viscosity of poise.

64. The method of claim 45, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

65. The method of claim 45, wherein the tetrafluoroethylene polymer has a 11 Melt creep viscosity of poise.

66. The method of claim 45, wherein the tetrafluoroethylene polymer has a molecular weight of at least about 4.0×10 11 Melt creep viscosity of poise.

67. The method of claim 45, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 30 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

68. The method of claim 45, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 40 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

69. The method of claim 45, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 50 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

70. The method of claim 45, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 60 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

71. The method of claim 45, wherein the elastomeric fluoropolymer has a Mooney viscosity of at least about 70 MU measured according to ASTM D1646, Condition ML 1+10 (121°C).

72. The method of claim 45 wherein the elastomeric fluoropolymer is a vinylidene fluoride elastomeric fluoropolymer.

73. The method of claim 45 wherein the vinylidene fluoride elastomeric fluoropolymer comprises a copolymer of vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene.

74. The method of claim 45, wherein the tetrafluoroethylene polymer is a tetrafluoroethylene homopolymer.

75. The method of claim 45, wherein the tetrafluoroethylene polymer is a polymer having a molecular weight of at least about 4.0×10 11 The elastomeric fluoropolymer is a tetrafluoroethylene homopolymer having a melt creep viscosity of at least about 150 MU as measured according to ASTM D1646 under condition ML 1+10 (121° C.), and the elastomeric fluoropolymer is a copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene having a Mooney viscosity of at least about 17 MU as measured according to ASTM D1646 under condition ML 1+10 (121° C.).