Atomizing core, atomizer and electronic atomizing device

By using porous glass ceramic matrix and metal heating body in the electronic cigarette atomization core, a controllable pore structure is formed, which solves the problem of low atomization efficiency of existing ceramic matrix and achieves the effect of efficient atomization and long life.

CN119054962APending Publication Date: 2024-12-03SMOORE INTERNATIONAL HOLDINGS LIMITED
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310645427.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The pore structure of the porous ceramic matrix of the existing electronic cigarette atomization core is uncontrollable, resulting in low atomization efficiency.

Method used

A porous glass ceramic matrix is ​​used to form a porous structure with openings by sintering glass ceramic bubbles to ensure that the porous structure is controllable and combined with a metal heating body to improve atomization efficiency.

Benefits of technology

It achieves efficient atomization effect, avoids the accumulation of smoke and scale, extends service life, and ensures consistency of taste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054962A_ABST
    Figure CN119054962A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic atomization, in particular to an atomization core, an atomizer and an electronic atomization device. The invention provides an atomizing core. The atomizing core comprises a porous base body and a heating body. The porous substrate is a porous glass ceramic substrate, and the porous glass ceramic substrate comprises a plurality of glass ceramic bubbles; wherein adjacent glass ceramic bubbles are directly bonded to each other by sintering; at least part of the glass ceramic bubbles have openings; the voids within the glass ceramic bubbles having openings communicate with each other through the openings to form pores that extend through the porous glass ceramic substrate and up to the surface of the porous glass ceramic substrate. According to the porous matrix and the atomization core prepared through the glass bubbles, the pore structure is controllable, and the atomization efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic atomization, and in particular to an atomization core, an atomizer and an electronic atomization device. Background Art

[0002] As a good substitute for traditional cigarettes, common e-cigarettes with e-liquid are generally composed of three parts: a cigarette rod, an atomizer core and an atomizer chamber. The battery is set in the cigarette rod, and the atomizer core is set in the e-liquid chamber. Among them, the atomizer core is the heart of the entire e-cigarette. The e-liquid is atomized into smoke through the atomizer core, and the atomized gas is exported to the mouthpiece. Compared with traditional cigarettes, the advantage of e-cigarettes is that they reduce harmful substances such as tar and CO in the smoke, and finally achieve the purpose of replacing cigarettes or relieving addiction, and reduce the absorption of harmful substances. At present, the atomization method of commercially available e-cigarettes is mainly resistive heating atomization, which atomizes the e-cigarette oil by heating the atomizer core. The existing atomizer core usually includes a porous matrix and a heating element. The porous matrix usually adopts materials with a porous structure such as cotton core and porous ceramics to achieve the function of guiding the atomization medium to the heating element.

[0003] However, ceramic materials are usually prepared using materials such as diatomaceous earth, and the porous matrix prepared therefrom has problems such as uncontrollable pore structure and low atomization efficiency. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem of low atomization efficiency in the prior art, and further provide an atomization core, an atomizer and an electronic atomization device.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme:

[0006] The present invention provides an atomizer core, which includes a porous matrix and a heating element;

[0007] The porous matrix is ​​a porous glass ceramic matrix, and the porous glass ceramic matrix includes a plurality of glass ceramic bubbles;

[0008] Therein, adjacent glass-ceramic bubbles are directly bonded to each other by sintering;

[0009] At least some of the glass-ceramic bubbles have openings;

[0010] The cavities within the glass-ceramic bubbles having openings are interconnected through the openings to form pores, which extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

[0011] Preferably, the thermal expansion coefficient of the porous glass-ceramic matrix is ​​10×10 -6 -21×10 -6 / ℃.

[0012] Preferably, the crystallinity of the glass ceramic bubbles is greater than 45-95%.

[0013] Preferably, the opening ratio of the glass ceramic bubbles in the porous glass ceramic matrix is ​​greater than 80%.

[0014] Preferably, the porosity of the porous glass-ceramic matrix is ​​50-90%;

[0015] Preferably, the porosity of the porous glass-ceramic matrix is ​​60-80%.

[0016] Preferably, the porous glass-ceramic matrix further comprises pores formed by a pore former.

[0017] Preferably, in the porous glass-ceramic matrix, the pore volume formed by the glass-ceramic bubbles with openings accounts for more than 70% of the total pore volume of the porous glass-ceramic matrix.

[0018] Preferably, the average pore size in the porous glass-ceramic matrix is ​​10-60 μm.

[0019] Preferably, the heating element is selected from at least one of a metal heating wire, a metal heating mesh, and a metal heating film;

[0020] The heating element is disposed on at least one surface of the porous glass-ceramic substrate;

[0021] Optionally, the metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

[0022] The present invention provides an atomizer, wherein the atomizer comprises the atomization core as described above.

[0023] The present invention provides an electronic atomization device, which includes the atomizer as described above and also includes a battery assembly.

[0024] Beneficial effects of the present invention:

[0025] The present invention provides an atomizer core, the atomizer core comprising a porous matrix and a heating element; the porous matrix is ​​a porous glass ceramic matrix, the porous glass ceramic matrix comprising a plurality of glass ceramic bubbles; wherein adjacent glass ceramic bubbles are directly bonded to each other by sintering; at least some of the glass ceramic bubbles have openings; the cavities in the glass ceramic bubbles with openings are interconnected through the openings to form pores, the pores extending through the porous glass ceramic matrix and reaching the surface of the porous glass ceramic matrix. The present invention forms a porous matrix and an atomizer core with a specific structure through glass ceramic bubbles, and the pore structure is controllable and the atomization efficiency is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 A physical picture of the atomizer core of Example 1 of the present invention;

[0028] Figure 2 A surface SEM image of the porous ceramic substrate of the atomizer core of Example 1 of the present invention;

[0029] Figure 3 A cross-sectional SEM image of the porous ceramic substrate of the atomizer core of Example 1 of the present invention;

[0030] Figure 4 Temperature field distribution diagram of the atomizer core of Example 1 of the present invention;

[0031] Figure 5 Statistical diagram of the temperature area of ​​the atomizer core in Example 1 of the present invention;

[0032] Figure 6 Schematic diagram of the fouling of the atomizer core in Example 1 of the present invention;

[0033] Figure 7 Schematic diagram of the atomizer of the present invention;

[0034] Figure 8 Schematic diagram of the electronic atomization device of the present invention;

[0035] Figure numerals: 1-atomizer, 2-battery assembly. DETAILED DESCRIPTION

[0036] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0037] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0038] The main atomization method of commercially available electronic cigarettes is resistance heating atomization, which atomizes the electronic cigarette oil through the heat of the atomizer core. The existing atomizer core usually includes a porous matrix and a heating element. The porous matrix usually uses materials with a porous structure such as cotton core and porous ceramics to achieve the function of guiding the atomized medium to the heating element.

[0039] However, ceramic materials are usually prepared using materials such as diatomaceous earth, and the pore structure of the porous matrix prepared therefrom is uncontrollable and the atomization efficiency is poor.

[0040] To this end, the present invention provides an atomizer core, the atomizer core includes a porous matrix and a heating element; the porous matrix is ​​a porous glass ceramic matrix, and the porous glass ceramic matrix includes a plurality of glass ceramic bubbles; wherein adjacent glass ceramic bubbles are directly bonded to each other by sintering; at least some of the glass ceramic bubbles have openings; the holes in the glass ceramic bubbles with openings are interconnected through the openings to form pores, and the pores extend through the porous glass ceramic matrix and reach the surface of the porous glass ceramic matrix. The inventors have found that the porous glass ceramic matrix with a specific structure formed by glass ceramic bubbles has a controllable pore structure, good atomization efficiency, and is not easy to produce soot, does not affect the taste, and can improve the service life.

[0041] In some optional embodiments, the thermal expansion coefficient of the porous glass-ceramic matrix is ​​10×10 -6 -21×10 -6 / ℃. For example, the thermal expansion coefficient of the porous glass-ceramic matrix can be selected to be 10×10 -6 / ℃、11×10 -6 / ℃、12×10 -6 / ℃、13×10 -6 / ℃、14×10 -6 / ℃、15×10 -6 / ℃、16×10 -6 / ℃、17×10 -6 / ℃、18×10 -6 / ℃、19×10 -6 / ℃、20×10 -6 / ℃、21×10 -6 / ℃. The inventors found that the thermal expansion coefficient is 10×10 -6 -21×10 -6 / ℃ porous glass ceramic matrix can cooperate well with the heating element to avoid the difference between the two affecting the service life. At the same time, the thermal expansion coefficient changes less with temperature, which is conducive to the stability of the pore structure at different temperatures, stable liquid supply, stable and consistent atomization volume, and consistent taste. At the same time, it avoids failures such as cracks under thermal shock and increases the service life of the atomizer core.

[0042] The raw materials used in the present invention include glass bubbles with cavitation structure, also known as hollow glass "microspheres", which can be obtained commercially. In the preparation process of the present invention, the raw glass bubbles are sintered to form glass ceramic bubbles with openings of a certain crystallinity. In some optional embodiments, the crystallinity of the glass ceramic bubbles is 45-95%. For example, it can be selected that the crystallinity of the glass ceramic bubbles is 45%, 47%, 51%, 53%, 55%, 58%, 60%, 61%, 63%, 64%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%. Optionally, the raw glass bubbles may also have a certain degree of crystallinity, that is, the raw glass bubbles may be glass or glass ceramics.

[0043] In some optional embodiments, the opening rate of the glass ceramic bubbles in the porous glass ceramic matrix is ​​greater than 80%. The opening rate refers to the ratio of the volume of pores that are interconnected and can be used for liquid conduction to the total pore volume of the porous glass ceramic matrix. In the present invention, since the pore structure mainly comes from the cavity structure of the monomer glass bubble, therefore, in some embodiments of the present invention, the opening rate can be understood as the ratio of the number of glass ceramic bubbles with openings after sintering and the total number of glass bubbles before sintering. For example, it can be selected that the opening rate of the glass ceramic bubbles in the porous glass ceramic matrix is ​​80.1%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%. The inventor analyzed that: the higher the opening rate, the more conducive it is to form an interconnected pore structure, which can achieve better storage and conduction of liquid atomized medium.

[0044] In some optional embodiments, the porosity of the porous glass-ceramic matrix is ​​50-90%; for example, the porosity of the porous glass-ceramic matrix can be selected to be 50%, 51%, 52%, 53%, 55%, 58%, 59%, 60%, 61%, 63%, 65%, 67%, 68%, 69%, 70%, 71%, 73%, 75%, 77%, 79%, 80%, 81%, 83%, 85%, 88%, 90%. Preferably, the porosity of the porous glass-ceramic matrix is ​​60-80%. In some embodiments, the pores of the porous glass-ceramic matrix are completely formed by glass-ceramic bubbles with openings. In other embodiments, the pores of the porous glass-ceramic matrix include pores formed by glass-ceramic bubbles with openings, and also include pores formed by pore-forming agents. Further, in the porous glass-ceramic matrix, the pore volume formed by the glass-ceramic bubbles with openings accounts for more than 70% of the total pore volume of the porous glass-ceramic matrix. For example, it can be selected that the pore volume formed by the glass-ceramic bubbles with openings accounts for 70.1%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100% of the total pore volume of the porous glass-ceramic matrix. It should be noted that the porosity of the porous glass-ceramic matrix can be controlled and adjusted by the selection of raw material glass bubbles on the one hand, and can also be adjusted by appropriately adding a certain proportion of pore-forming agents during the preparation process. It can be understood that for a monomer glass bubble, the ratio of the volume of its internal cavities to the overall volume of the monomer glass bubble determines its density, so a glass bubble monomer of a specific density can be screened out by a liquid of appropriate density. Glass bubbles with this specific density can be used to prepare a porous glass-ceramic matrix with a corresponding porosity. It can be understood that if the density of a monomer glass bubble is too small, that is, its wall thickness is smaller, its strength will be reduced. Therefore, in the case of ensuring its strength requirements, it is impossible to increase the porosity by simply increasing the proportion of its cavities. Therefore, the inventor can further increase its porosity by adding a pore-forming agent while ensuring the overall strength of the glass bubble and the porous glass-ceramic matrix after molding.

[0045] In some optional embodiments, the pores in the porous glass-ceramic matrix have a pore size of 10-60 μm. For example, the pores in the porous glass-ceramic matrix can be selected to have a pore size of 10 μm, 13 μm, 15 μm, 19 μm, 20 μm, 25 μm, 27 μm, 30 μm, 35 μm, 36 μm, 40 μm, 43 μm, 48 μm, 50 μm, 52 μm, 58 μm, and 60 μm. The pore size range is moderate, and it has both the effect of guiding and locking liquid. It should be noted that the pore size of the porous glass-ceramic matrix can also be controlled and adjusted by the selection of raw glass bubbles. By appropriate screening, the raw glass bubbles of the required particle size can be obtained; combined with the appropriate volume proportion of the cavities described above, the pore size of the required raw glass bubble cavities can be obtained. Through suitable raw glass bubbles and preparation processes, the pore structure of the porous glass-ceramic matrix is ​​controllable.

[0046] The present invention does not specifically limit the specific form and material of the heating element. For example, the heating element can be selected from at least one of a metal heating wire, a metal heating mesh, and a metal heating film. In an optional embodiment, the heating element is disposed on at least one surface of the porous glass-ceramic substrate; further, the metal heating film is selected from at least one of stainless steel and a nickel-containing alloy. In an optional embodiment, the heating element is a metal heating film.

[0047] In some optional embodiments, the heating element is disposed on at least one surface of the porous glass-ceramic substrate in a manner including at least one of printing, welding, evaporation, and deposition. For example, it is possible to print the heating element slurry on the substrate and sinter it at a preset temperature. It is possible to weld the heating element or heating net on the substrate. It is possible to evaporate / deposit the heating element on the substrate by physical vapor deposition (PVD) or chemical vapor deposition (CVD).

[0048] In some optional embodiments, the method further includes coating the electrode slurry on at least one end of the heating element and sintering the slurry into a shape.

[0049] The present invention is further described below in conjunction with the preparation method.

[0050] In some optional embodiments, the method for preparing the atomizer core comprises the following steps:

[0051] 1) mixing raw glass bubbles with a binder, a lubricant and water and extruding the mixture to obtain a green body;

[0052] 2) subjecting the green body in step 1) to a first sintering, a second sintering and a third sintering to obtain a porous glass-ceramic matrix;

[0053] 3) The raw material of the heating element is prepared on the porous glass ceramic substrate in step 2) and sintered into shape.

[0054] In some optional embodiments, in step 1): the binder can be an organic binder; specifically, the binder is selected from at least one of methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose; the lubricant can be an aliphatic hydrocarbon lubricant, such as paraffin, metal stearate; specifically, the lubricant is sodium stearate.

[0055] In some optional embodiments, the pressure of the extrusion molding in step 1) is 1-30 bar. Most of the glass bubbles do not break during the extrusion molding process, and the single glass bubble maintains a complete spherical shape. Therefore, the extrusion molding pressure can be appropriately adjusted according to the compressive strength of the selected glass bubble.

[0056] In some optional embodiments, the first temperature of the first sintering in step 2) is at least 200° C., such as 300° C. to 400° C., and / or the first residence time is at least 1 minute, such as 1 to 10 hours. During the sintering process at this temperature, substances such as solvents and binders in the green body are removed.

[0057] In some optional embodiments, the second temperature of the second sintering is greater than 400°C and less than the softening point of the glass of the glass bubble; for example, 500°C, 600°C, 700°C, etc., and the second residence time is at least 1 minute, for example, 1 to 10 hours. The second temperature is higher than 400°C and lower than the softening point of the glass of the glass bubble. The purpose is to keep the original shape of the blank unchanged. At the same time, since the temperature is already higher than 400°C, the glass component in the glass bubble begins to undergo a phase change, and the disordered glass phase partially crystallizes into a crystalline phase within this temperature range. The glass bubble is transformed into a glass ceramic bubble or the proportion of the crystalline phase in the glass bubble begins to increase. At the same time, due to this transformation, some glass bubbles begin to break and have at least one opening. Therefore, the sintering time within this temperature range can be appropriately adjusted to adjust the crystallinity of the porous glass ceramic. It can be understood that the raw glass bubble itself can also contain a certain proportion of crystalline phases, which can shorten the sintering time in this process.

[0058] In some optional embodiments, the third temperature of the third sintering is greater than the softening point of the glass. Specifically, the softening point temperature of the glass is less than 900°C. The third residence time can be at least 1 minute, for example, 1 to 10 hours. At this temperature, the glass component has fluidity, so the adjacent glass-ceramic bubbles are directly bonded to each other, and the glass-ceramic bubbles are bonded to form a porous glass-ceramic matrix of an integral structure; at the same time, because the glass-ceramic bubbles still have crystalline phase components, the crystalline phase components serve as a skeleton so that their morphology does not collapse, and they still maintain a basically complete morphology. In addition, the glass-ceramic bubbles further crack to form a large number of openings, which are interconnected to form pores, and the pores extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

[0059] The third temperature is higher than the softening point of the glass of the glass bubble. The glass ceramic bubble is heated to at least the softening temperature of the amorphous glass, so that most of the glass ceramic bubbles are opened due to the expansion of the gas in the bubble, and the adjacent glass ceramic bubbles are sintered together by heating to form a bond. From the overall point of view, the bonded open glass ceramic bubbles form pores in the porous glass ceramic matrix, which can be used in atomizers and electronic atomization devices to effectively improve the atomization efficiency and liquid guiding effect.

[0060] In some optional embodiments, the mass ratio of glass bubbles to binder, lubricant and water is (100-200): (10-50): (1-10): (45-150).

[0061] In some optional embodiments, in step 3), the raw material of the heating element may be at least one of electronic paste (metal paste), heating wire or heating mesh. The electronic paste may be directly applied to the surface of the porous glass-ceramic substrate in a preset shape by silk-screen printing, and sintered at a preset temperature. The sintering temperature may be adaptively adjusted according to the type of the binder phase and the metal component in the electronic paste, and the sintering temperature is usually 400-800°C.

[0062] In some optional embodiments, the glass component in the glass bubble may be soda-lime silicate glass, borosilicate glass or other glass. Specifically, the glass component may include: SiO 2 74-85%, CaO 6.5-10%, B 2 O 3 5-9%, Al 2 O 3 0.4-2%, Fe 2 O 3 0.01-1%, Na 2 O 1-3%, K 2 O 0.1-0.5%.

[0063] In some optional embodiments, step 1) further includes adding a pore former. Optionally, the pore former is selected from at least one of starch, polymethyl methacrylate (PMMA), polystyrene (PS), and graphite. Optionally, the particle size range of the pore former can be 1-150 μm. It can be understood that the addition of the pore former can further improve the porosity of the porous glass ceramic matrix while ensuring the strength of the raw glass bubble.

[0064] In some optional embodiments, step 1) further includes a second inorganic material. The second inorganic material may be at least one of clay, talc, silica, and alumina. The melting point or softening point of the above materials is higher than the softening point of the glass in the glass bubble.

[0065] In some optional embodiments, the mass ratio of glass bubbles to binder, slip agent, water, pore former, and second inorganic material is (100-200): (10-50): (1-10): (45-150): (0-70): (0-9).

[0066] like Figure 7 As shown, the present invention also provides an atomizer, wherein the atomizer includes the atomizer core described above. The atomizer includes a shell, and a liquid storage tank and an atomization cavity are formed in the shell. The liquid storage tank is used to store liquid atomization medium, and the atomization cavity is used to accommodate the atomization core described above. The atomization core can atomize the liquid atomization medium.

[0067] like Figure 8 As shown, the present invention also provides an electronic atomization device, which includes the above-mentioned atomizer 1 and a battery assembly 2. The battery assembly and the atomizer can be an integrated structure or a detachable structure. The battery assembly is used to power the atomizer according to a preset mode, so that the atomizer atomizes the liquid atomization medium according to the preset mode.

[0068] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed by the present invention.

[0069] The following embodiments of the present invention all use raw glass bubbles of the same composition, the raw glass bubbles are soda-lime silicate glass, and the raw material particle size parameters are: D10=18.61μm, D50=39.38μm, D90=69.47μm, and the porosity of the glass bubble monomer is 84.8%; the main components of the raw glass bubbles are Si: 41.647wt%, O: 49.375wt%, Na: 3.778wt%, Ca: 4.619wt%, Mg: 0.201wt%, and Al: 0.379wt%.

[0070] Example 1

[0071] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0072] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate and 48 g of water and extruded to obtain a green body at a molding pressure of 23 bar;

[0073] 2) subjecting the green body in step 1) to a first sintering, a second sintering and a third sintering to obtain a porous glass ceramic substrate, wherein the first sintering temperature is 220° C., the first sintering time is 2 hours, the second sintering temperature is 600° C., the second sintering time is 2 hours, the third sintering temperature is 1200° C., the third sintering time is 1 hour, and finally, the green body is naturally cooled in the furnace to obtain a porous glass ceramic substrate;

[0074] 3) Printing the heating element slurry on the porous glass ceramic substrate in step 2), sintering and forming, the sintering temperature is 600° C., and the sintering time is 1 hour to obtain the atomizing core. The heating element slurry is stainless steel.

[0075] like Figure 1 As shown, the atomizer core prepared in this embodiment has a porous matrix that is a porous glass-ceramic matrix, and the porous glass-ceramic matrix includes a plurality of glass-ceramic bubbles; wherein adjacent glass-ceramics are directly bonded to each other by sintering the bubbles; some of the glass-ceramic bubbles have openings; the cavities in the glass-ceramic bubbles with openings are interconnected through the openings to form pores, and the pores extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

[0076] Example 2

[0077] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0078] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 25 g of a pore former and 67 g of water, and the mixture was extruded to obtain a green body at a molding pressure of 12 bar; the pore former was polystyrene with an average particle size of 50 μm.

[0079] Step 2) and step 3) are the same as in Example 1.

[0080] Example 3

[0081] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0082] 1) 100 g of glass bubbles, 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 4 g of a second inorganic material, 50 g of a pore former, and 75 g of water are mixed and extruded to obtain a green body at a molding pressure of 15 bar. The second inorganic material is clay, the pore former is polymethyl methacrylate (PMMA), and the average particle size of the pore former is 50 μm.

[0083] Step 2) and step 3) are the same as in Example 1.

[0084] Test Case

[0085] The porous glass ceramic substrate of the atomizer core of the embodiment of the present invention was tested for the opening ratio, thermal expansion coefficient, porosity and pore size. The test method or standard for the opening ratio is based on GB / T 10799-2008, the test for the thermal expansion coefficient is performed using a thermal expansion coefficient meter, and the test method for the porosity and pore size is a mercury intrusion method (the test equipment is a mercury intrusion instrument).

[0086] The results of the average pore size, porosity and opening ratio of Examples 1 to 3 are shown in Table 1.

[0087] Table 1 Test results of porous glass ceramic substrates in the embodiment

[0088] Example Average pore size (μm) Porosity (%) Opening rate (%) Example 1 18.4 62.01 98 Example 2 21.77 77.06 96 Example 3 20.44 76.35 87

[0089] The thermal expansion coefficients of Example 1 and Example 2 are shown in Table 2.

[0090] Table 2 Test results of thermal expansion coefficient of porous glass ceramic matrix in Example

[0091]

[0092] like Figure 2 and Figure 3 As shown, Figure 2 This is the surface SEM image of Example 1. Figure 3 The SEM image of the cross section of the interior thereof shows that the porous glass-ceramic matrix has a rich, developed and interconnected pore structure inside, and extends to the surface of the porous glass-ceramic matrix, and the surface also has a rich pore structure.

[0093] The atomizer core in Example 1 was used to test the smoke volume, soot, lifespan, and temperature field of the atomizer core. At the same time, the atomizer core in Example 1 was used to conduct a puffing experiment to test the puffing taste. Among them, the test method of the smoke volume is that each puffing process (i.e., each puff) includes: puffing for 3S and then pausing for 8S, testing the smoke volume of each puffing process, and taking the average value by statistics. The temperature field of the atomizer core uses an infrared thermometer to obtain the distribution of the temperature field, and then the distribution statistics of the temperature field are performed. After the preset number of puffs (the preset number of puffs in this application is 500 puffs), the soot on the surface of the atomizer core is observed to determine the deposition of the soot. During the preset number of puffs, whether there is a failure situation in this process is tested, and its lifespan is statistically recorded, wherein the failure situations mainly include: 1. The resistance value of the atomizer core changes significantly abnormally (such as: the resistance value increases significantly due to the breakage and shedding of the heating element); 2. The amount of fog output is less than half of the initial atomization amount. The above test conditions are 6.5W power, bare chip (not assembled into an atomizer); the taste test assembles the atomizer core into an atomizer.

[0094] The puffing taste is determined by the tester's judgment of whether there is an abnormal taste such as a burnt smell during the preset number of puffs.

[0095] The above-mentioned tests on soot, smoke volume, lifespan and atomizer core were respectively tested with two different flavors of e-liquids: fruit (watermelon) flavored e-liquid (e-liquid a) and tobacco flavored e-liquid (e-liquid b). As shown in Table 3, the temperature field, smoke volume, soot, taste, lifespan (whether it fails after 500 puffs) of the atomizer core of the embodiment of the present invention tested with e-liquid a, and the smoke volume tested with e-liquid b.

[0096] Table 3 Test results of the embodiment of the atomizer core

[0097]

[0098] As shown in Table 3, within the preset number of 500 puffs, the atomization volume of the atomizer core of the present invention is large, which meets the preset service life requirement of 500 puffs, has a good taste, and has no burnt smell.

[0099] like Figure 4-Figure 6As shown, they are respectively the temperature field distribution diagram, the temperature zone area statistics diagram and the scaling diagram of Example 1. It should be noted that the liquid atomization matrix (smoke oil) usually includes 1-50 parts of propylene glycol (PG), 30-50 parts of vegetable glycerin (VG), 0-20 parts of edible flavors, 0-5 parts of nicotine / nicotine salts, etc. Among them, the boiling point of propylene glycol (PG) is about 188.2°C, and the boiling point of vegetable glycerin (VG) is about 290°C; therefore, the effective atomization temperature range of the liquid atomization matrix should usually be at least greater than 190°C, and the ideal optimal atomization temperature range is slightly different depending on the added proportion and type of vegetable glycerin (VG) and edible flavors. In the present invention, Figure 5 It can be seen that for e-liquid a, the temperature of the main atomization area during the atomization process of the atomizer core is 220-310℃, and the local high temperature is 310-340℃. The temperature range is concentrated in the high-efficiency atomization range, which is conducive to improving the atomization efficiency and is not easy to scale. For e-liquid b: the temperature of the main atomization area is 220-370℃, the local high temperature is 370-400℃, and the areas of several temperature ranges such as 220-250℃, 250-280℃, 280-310℃, and 310-340℃ are basically the same, which shows that it has a certain temperature gradient. This kind of gradient temperature distribution can better stimulate the richness of the layered e-liquid, making the taste rich and improving the user experience.

[0100] like Figure 6 As shown, the distribution of soot on the atomization surface of the atomization core of Example 1 after 500 puffs of the test. After 500 puffs of smoking, the soot deposition on the atomization surface of the e-liquid a is very small. The reason is that the efficient atomization temperature range of this atomization medium is low, it is not easy to scale, and the atomization efficiency is high. After 500 puffs of smoking, there is a small amount of scale on the atomization surface of the e-liquid b. The reason is that the efficient atomization temperature range of this atomization medium is high, and the temperature zone distribution has a certain gradient, which can improve the taste. Both e-liquids are still not invalid after 500 puffs of the test, and their lifespan and reliability are good.

[0101] The inventors analyzed and believed that: the temperature field of the atomizer core provided by the present invention is concentrated in the high-efficiency area, and there is a certain temperature field gradient; therefore, the atomization efficiency is high, it is not easy to scale, and does not produce dry burning. At the same time, it has a rich taste layer and no burnt smell. At the same time, the internal pore channels are well developed, which can quickly supply the smoke oil to the atomization surface, avoiding local high temperature and dry burning of the product due to insufficient liquid supply. At the same time, due to the use of glass bubble sintering preparation and certain process control, the glass is transformed into glass ceramics (i.e., crystallization), so that the volume of the porous glass ceramic matrix is ​​stable and the thermal expansion coefficient is in a suitable range. Avoid the breakage and failure of the heating element due to excessive volume changes during use, and increase the service life of the atomizer core. Specifically, the pore structure of the porous glass ceramic matrix has a high opening rate, very few closed pores, and a good oil conduction effect. Further analysis shows that the reason for the high opening rate is that the opening of the glass bubble monomer is stable, and because of its high crystallinity and the particles that have been crystallized into crystals, its melting point is higher and it will not soften, so it can serve as a skeleton to keep the shape of the entire matrix unchanged. Therefore, it avoids collapse during the sintering process, ensures that the pores are not destroyed, and maintains a good skeleton state, thereby achieving better oil conduction effect and better appearance stability, and improving atomization efficiency and service life.

[0102] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. An atomizer core, characterized in that: The atomizing core comprises a porous matrix and a heating element; The porous matrix is ​​a porous glass ceramic matrix, and the porous glass ceramic matrix includes a plurality of glass ceramic bubbles; Therein, adjacent glass-ceramic bubbles are directly bonded to each other by sintering; At least some of the glass-ceramic bubbles have openings; The cavities within the glass-ceramic bubbles having openings are interconnected through the openings to form pores, which extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

2. The atomizer core according to claim 1, characterized in that: The thermal expansion coefficient of the porous glass ceramic matrix is ​​10×10 -6 -21×10 -6 / ℃.

3. The atomizer core according to claim 1 or 2, characterized in that: The crystallinity of the glass ceramic bubbles is 45-95%.

4. The atomizer core according to any one of claims 1 to 3, characterized in that: The opening ratio of the glass ceramic bubbles in the porous glass ceramic matrix is ​​greater than 80%.

5. The atomizer core according to any one of claims 1 to 4, characterized in that: The porosity of the porous glass-ceramic matrix is ​​50-90%; Preferably, the porosity of the porous glass-ceramic matrix is ​​60-80%.

6. The atomizer core according to any one of claims 1 to 5, characterized in that: The porous glass-ceramic matrix further includes pores formed by a pore former.

7. The atomizer core according to claim 6, characterized in that: In the porous glass-ceramic matrix, the pore volume formed by the glass-ceramic bubbles with openings accounts for more than 70% of the total pore volume of the porous glass-ceramic matrix.

8. The atomizer core according to any one of claims 1 to 7, characterized in that: The average pore size of the porous glass-ceramic matrix is ​​10-60 μm.

9. The atomizer core according to any one of claims 1 to 8, characterized in that: The heating element is selected from at least one of a metal heating wire, a metal heating mesh, and a metal heating film; The heating element is disposed on at least one surface of the porous glass-ceramic substrate; Optionally, the metal heating film is selected from at least one of stainless steel and nickel-containing alloy.

10. An atomizer, characterized in that: The atomizer comprises the atomizer core according to any one of claims 1 to 9.

11. An electronic atomization device, characterized in that: The electronic atomization device comprises the atomizer according to claim 10, and further comprises a battery assembly.

Citation Information

Cited By

  • Atomization core, atomizer and electronic atomization device

    EP4721602A1