Maleic anhydride hydrogenation catalyst as well as preparation method and application thereof
By adding rhenium compounds to the catalyst, a highly active cRe2O7/CuM1aM2bOx catalyst was prepared, which solved the problem of low conversion and selectivity of existing catalysts at low temperatures, and achieved efficient catalytic reactions at low temperatures and high airspeeds, which significantly improved Selectivity and yield of 1,4-butanediol.
Patent Information
- Application Number
- CN202310642175.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
AI Technical Summary
When existing catalysts are used to prepare 1,4-butanediol at low temperatures, the liquid time space speed is small and the conversion and selectivity are low, making it difficult to maintain high efficiency at high aerial speeds.
Using the rhenium-containing composite metal oxide catalyst cRe2O7/CuM1aM2bOx, a high-activity catalyst is prepared by combining the compounds of metal Cu, M1, M2 with Re2O7 or HReO4, and the catalyst is reduced under specific conditions to improve the activity of the catalyst and stability.
The conversion rate of maleic anhydride and the selectivity of 1,4-butanediol are significantly improved at lower temperatures, and excellent technical effects are maintained under high airspeed conditions, achieving efficient catalytic reactions.
Smart Images

Figure BDA0004261862500000061 
Figure BDA0004261862500000071 
Figure BDA0004261862500000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic materials, and particularly relates to a maleic anhydride hydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] 1,4-Butanediol is an important organic chemical raw material, primarily used in the production of polybutylene terephthalate (PBT), polyurethane, γ-butyrolactone, and tetrahydrofuran. γ-Butyrolactone is an excellent high-boiling-point solvent and an important raw material for fine chemicals and organic chemicals.
[0003] There are many methods for preparing 1,4-butanediol and γ-butyrolactone. The most commonly used method is to prepare 1,4-butanediol and / or γ-butyrolactone from maleic anhydride and / or maleic acid and / or succinic anhydride and / or succinic acid and / or their alkyl esters by gas phase hydrogenation.
[0004] SU 1022969 reported the use of CuO-Cr2O3-ZnO / Al2O3 as catalyst, 260℃-280℃, liquid hourly space velocity of 0.2-0.3h -1 , dibutyl maleate was hydrogenated to γ-butyrolactone with a conversion rate of 97 mol% and a selectivity of γ-butyrolactone of 85 mol%.
[0005] CS 171623 reported that γ-butyrolactone was prepared by hydrogenation of dibutyl maleate or succinate using CuO-Cr2O3-ZnO / silica gel as a catalyst at 250-270°C and a hydrogen / ester molar ratio of 30:1. The yield of γ-butyrolactone was 70 mol%.
[0006] WO8607358 reports a method for preparing γ-butyrolactone from C4 carboxylic acid esters using a two-stage hydrogenation process using a Cu-Cr-Ba or Mn catalyst at 170-260°C, 11-30 bar, and a hydrogen / ester ratio of 50-1000:1 (mol). However, this method has low feed space velocity and low selectivity for preparing γ-butyrolactone.
[0007] EP143634 discloses a method for producing 1,4-butanediol by a two-stage gas phase hydrogenation process using a Cu-Cr-Mn-Ba mixed oxide as a catalyst and maleic acid ester as a raw material. Summary of the Invention
[0008] The inventors discovered through experiments that, when using existing catalysts to produce 1,4-butanediol from maleic anhydride, the liquid hourly space velocity of the maleic anhydride as a raw material is low. Increasing the space velocity of the maleic anhydride significantly decreases the feedstock conversion rate and the selectivity for 1,4-butanediol. Furthermore, while it is well known in the art that low temperatures are beneficial for improving the selectivity for 1,4-butanediol, the low-temperature liquid hourly space velocity and feedstock conversion rate of existing catalysts are generally low. Therefore, there is an urgent need to develop a maleic anhydride hydrogenation catalyst for use at low temperatures and high space velocities with 1,4-butanediol as the target product.
[0009] The present invention provides a rhenium-containing composite metal oxide catalyst cRe2O7 / CuM1 for hydrogenation of maleic anhydride a M2 b O x ,
[0010] wherein M1 and M2 each independently represent Al, Ti, Zr, Zn, K, Na, Ca, Mn, Mg, B, Se, Sb, P, C, Sn, Co, Fe, Ni, V, Cr, Mo, W, Si, Pd, Pt, Ag, Ru, Ga, In, Y, La, Ce, Nd or a rare earth metal;
[0011] a is selected from 0-4;
[0012] b is selected from 0-4;
[0013] x is the number of oxygen atoms that satisfy the valence state of each metal atom;
[0014] c is 0.01wt%-40wt%, preferably 0.01wt%-10wt%, more preferably 0.1wt%-4wt%;
[0015] c represents Re2O7 and CuM1 a M2 b O x weight percentage.
[0016] The second object of the present invention is to provide a method for preparing the above-mentioned catalyst, which specifically comprises the following steps:
[0017] (1) Dissolve or disperse the compound of metal Cu, M1, and M2 in water, add a precipitant, adjust the pH to precipitate, age, filter, collect the precipitate, dry, and calcine to obtain the composite oxide CuM1 a M2 b O x ;
[0018] (2) The composite oxide CuM1 prepared in step (1) a M2 b Ox Add acetone solution containing Re2O7, immerse and dry to obtain the catalyst cRe2O7 / CuM1 a M2 b O x .
[0019] The third object of the present invention is to provide another method for preparing the above-mentioned catalyst, which specifically comprises the following steps:
[0020] (a) dissolving or dispersing a compound of metal Cu, M1, and M2 in water, adding a precipitant, adjusting the pH to a point where precipitation occurs, aging, filtering, collecting the precipitate, drying, and calcining to obtain a composite oxide CuM1. a M2 b O x ;
[0021] (b) the composite oxide CuM1 prepared in step (a) a M2 b O x Adding aqueous solution containing HReO4, impregnating, drying, and calcining to obtain the catalyst cRe2O7 / CuM1 a M2 b O x .
[0022] A fourth object of the present invention is to provide use of the above catalyst or the catalyst prepared by the above preparation method in the hydrogenation of maleic anhydride to prepare 1,4-butanediol.
[0023] Beneficial effects:
[0024] The present invention is through the composite metal oxide CuM1 a M2 b O x By combining a catalyst with a small amount of a rhenium-containing compound, the catalyst exhibits higher activity (i.e., higher feedstock conversion) at lower temperatures in the hydrogenation of maleic anhydride to 1,4-butanediol compared to catalysts without rhenium compounds, further improving the selectivity and yield of 1,4-butanediol. This excellent technical effect is maintained even at higher space velocities. DETAILED DESCRIPTION
[0025] The following examples are further given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are only examples within a suitable range. That is, those skilled in the art can make selections within a suitable range based on the description herein, and are not limited to the specific values exemplified below.
[0026] The present invention provides a rhenium-containing composite metal oxide catalyst cRe2O7 / CuM1 for hydrogenation of maleic anhydride a M2 b O x ,
[0027] wherein M1 and M2 each independently represent Al, Ti, Zr, Zn, K, Na, Ca, Mn, Mg, B, Se, Sb, P, C, Sn, Co, Fe, Ni, V, Cr, Mo, W, Si, Pd, Pt, Ag, Ru, Ga, In, Y, La, Ce, Nd or a rare earth metal;
[0028] Preferably, M1 and M2 each independently represent Al, Ti, Zr, Zn, Mn, Co, Fe, Ni, Mg, La or Ce;
[0029] Further preferably, M1 and M2 each independently represent Zr, Zn, Mn, Al or Fe;
[0030] Still further preferably, M1 and M2 each independently represent Zr, Mn or Al;
[0031] a is selected from 0-4;
[0032] b is selected from 0-4;
[0033] x is the number of oxygen atoms that satisfy the valence state of each metal atom;
[0034] Preferably, x is selected from 1-3, preferably, x is selected from 2-3;
[0035] c is 0.01 wt% to 40 wt%, preferably 0.01 wt% to 10 wt%, more preferably 0.1 wt% to 4 wt%
[0036] According to a specific embodiment of the present invention, a and b are not 0 at the same time.
[0037] According to a specific embodiment of the present invention, the catalyst needs to be reduced before use. The reducing agent is a reducing gas, preferably H2 and / or CO. The reduction conditions are: the reduction pressure is 1.0-6.0 MPa, the reduction temperature is 250-300°C; the reducing gas flow rate is 50-200 ml / min / g catalyst.
[0038] The present invention provides a method for preparing the above catalyst, which specifically comprises the following steps:
[0039] (1) Dissolve or disperse the compound of metal Cu, M1, and M2 in water, add a precipitant, adjust the pH to precipitate, age, filter, collect the precipitate, dry, and calcine to obtain the composite oxide CuM1 a M2 b O x ;
[0040] Wherein, in the above step (1), the compound of metal Cu, M1, M2 is a soluble salt or oxide of metal Cu, M1, M2; preferably, it is a nitrate or hydrochloride; more preferably, it is a nitrate.
[0041] The precipitant is ammonia water, carbonate, bicarbonate, or soluble metal hydroxide, preferably ammonia water.
[0042] pH 3.0-10.0, preferably 5.0-9.0, more preferably 7±0.5;
[0043] The aging temperature is room temperature, and the aging time is 1-4 hours;
[0044] The drying temperature is 100-200°C and the drying time is 2-10 hours;
[0045] The calcination temperature is 300-600° C., and the calcination time is 2-30 hours.
[0046] (2) The composite oxide CuM1 prepared in step (1) a M2 b O x Add acetone solution containing Re2O7, immerse and dry to obtain catalyst cRe2O7 / CuM1 a M2 b O x ;
[0047] Wherein, in step (2), the dipping time is 1-25 hours; the drying temperature is 100-200° C., and the drying time is 1-20 hours.
[0048] The present invention provides another method for preparing the above catalyst, which specifically comprises the following steps:
[0049] (a) dissolving or dispersing a compound of metal Cu, M1, and M2 in water, adding a precipitant, adjusting the pH to a point where precipitation occurs, aging, filtering, collecting the precipitate, drying, and calcining to obtain a composite oxide CuM1. a M2 b O x ;
[0050] Wherein, in the above step (a), the compound of metal Cu, M1, and M2 is a soluble salt or oxide of metal Cu, M1, and M2; preferably a nitrate or a hydrochloride; more preferably a nitrate.
[0051] The precipitant is ammonia water, carbonate, bicarbonate, or soluble metal hydroxide, preferably ammonia water.
[0052] pH 3.0-10.0, preferably 5.0-9.0, more preferably 7±0.5;
[0053] The aging temperature is room temperature, and the aging time is 1-10 hours;
[0054] The drying temperature is 100-200°C and the drying time is 2-10 hours;
[0055] The calcination temperature is 300-600° C., and the calcination time is 2-30 hours.
[0056] (b) the composite oxide CuM1 prepared in step (a) a M2 b O x Adding aqueous solution containing HReO4, impregnating, drying, and calcining to obtain the catalyst cRe2O7 / CuM1 a M2 b O x .
[0057] Wherein, in the above step (b), the impregnation time is 10-25 hours; the drying temperature is 100-200° C., and the drying time is 1-20 hours; the roasting temperature is 300-400° C., and the roasting time is 1-10 hours.
[0058] The present invention provides use of the catalyst or the catalyst obtained by the preparation method in hydrogenating maleic anhydride to prepare 1,4-butanediol.
[0059] According to a specific embodiment of the present invention, the temperature of the hydrogenation reaction is 140-280°C, preferably 140-220°C, more preferably 160-190°C, and the reaction pressure is 1.0-10.0 MPa; preferably 1.0-7.0 MPa; the molar ratio of hydrogen to raw material is (60-400):1, preferably (100-250):1; when the solvent is added, the molar ratio of the raw material to the solvent is 0.1-5.0:1.
[0060] According to a specific embodiment of the present invention, the feed liquid hourly space velocity of the raw material maleic anhydride is 0.1-1.0h -1 , preferably 0.1-0.6h -1 , more preferably 0.1-0.2h -1 , more preferably 0.1-0.14h -1 .
[0061] According to one embodiment of the present invention, the catalyst is suitable for use with maleic anhydride and / or its monoesters and / or diesters. These raw materials can be fed together with one or more of γ-butyrolactone, tetrahydrofuran, and an alcohol, wherein the alcohol is a C1-C6 alcohol. The catalyst is particularly suitable for hydrogenating maleic anhydride to produce γ-butyrolactone, tetrahydrofuran, and 1,4-butanediol.
[0062] The following preparation examples 1-3 are examples of the preparation of the catalyst of the present invention
[0063] The sources of raw materials used in the present invention are shown in Table 1
[0064] Table 1
[0065] raw material source <![CDATA[Cu(NO3)2·3H2O]]> Beijing Chemical Plant, Chemically Pure <![CDATA[Zn(NO3)2·6H2O]]> Beijing Chemical Plant, Chemically Pure <![CDATA[ZrO(NO3)·2H2O]]> Beijing Chemical Plant, Chemically Pure <![CDATA[Na2CO3]]> Beijing Chemical Plant, Chemically Pure <![CDATA[Mn(NO3)2·4H2O]]> Beijing Chemical Plant, Chemically Pure
[0066] Preparation Example 1
[0067] 84.69 g of Cu(NO3)2·3H2O, 92.29 g of Zn(NO3)2·6H2O, and 19.7 g of ZrO(NO3)·2H2O were dissolved in 1000 ml of deionized water, stirred, and Na2CO3 was added dropwise until the pH was 7±0.5. After aging for 12 hours, the mixture was filtered and washed. After 6 washes with water, the precipitate was collected; dried at 120°C for 12 hours, and calcined at 450°C for 2.5 hours to obtain composite oxide catalyst A: CuZn 0.8 Zr 0.2 O 2.2 (Metal composition was analyzed by X-ray fluorescence analysis, and oxygen content was calculated, the same below).
[0068] 13 g of catalyst A was immersed in 15 ml of acetone solution containing 0.25 g of Re2O7 for 24 hours, dried at 120°C for 12 hours, and then heated to 150°C and dried for another 12 hours to obtain catalyst B: 1.9 wt% Re2O7 / CuZn 0.8 Zr 0.2 O 2.2 .
[0069] 13 g of catalyst A was immersed in 15 ml of acetone solution containing 0.17 g of Re2O7 for 24 hours, dried at 120°C for 12 hours, and then heated to 150°C and dried for another 12 hours to obtain catalyst B1: 1.3 wt% Re2O7 / CuZn 0.8 Zr 0.2 O 2.2 .
[0070] Preparation Example 2
[0071] 84.69 g of Cu(NO3)2·3H2O and 82.52 g of ZrO(NO3)·2H2O were dissolved in 1000 ml of deionized water, stirred and Na2CO3 was added dropwise until the pH was 7±0.5. After aging for 12 hours, the mixture was filtered and washed. After 6 washes with water, the precipitate was collected; dried at 120°C for 12 hours, and calcined at 450°C for 2.5 hours to obtain composite oxide catalyst C: CuZr 0.8 O 2.6 .
[0072] 13 g of catalyst C was immersed in 15 ml of acetone solution containing 0.25 g of Re2O7 for 24 hours, dried at 120°C for 12 hours, and then heated to 150°C and dried for another 12 hours to obtain catalyst D: 1.9 wt% Re2O7 / CuZr 0.8 O 2.6 .
[0073] Preparation Example 3
[0074] 84.69 g of Cu(NO3)2·3H2O, 110.44 g of Zn(NO3)2·6H2O, and 38.66 g of Mn(NO3)2·4H2O were dissolved in 1000 ml of deionized water, stirred, and Na2CO3 was added dropwise until the pH was 7±0.5. After aging for 12 hours, the mixture was filtered and washed. After washing with water 6 times, the precipitate was collected; dried at 120°C for 12 hours, and calcined at 450°C for 2.5 hours to obtain composite oxide catalyst E: CuZn1Mn 0.4 O 2.4 .
[0075] 13 g of catalyst C was immersed in 15 ml of acetone solution containing 0.25 g of Re2O7 for 24 hours, dried at 120°C for 12 hours, and then heated to 150°C and dried for another 12 hours to obtain catalyst F: 1.9 wt% Re2O7 / CuZn1Mn 0.4 O 2.4 .
[0076] The properties of the obtained catalysts are summarized in Table 2
[0077] Table 2
[0078]
[0079]
[0080] Example 1
[0081] 8.6 g of catalyst B with a particle size of 26-40 mesh was loaded into a stainless steel tubular reactor with an inner diameter of 10 mm. H2 was introduced at a flow rate of 25 ml / min at 300°C and 0.1 MPa. After reduction for 5 hours, maleic anhydride was used as the raw material. The reaction temperature was 175°C, the pressure was 6.0 MPa, the hydrogen anhydride molar ratio was 250:1, and the maleic anhydride liquid hourly space velocity was 0.14 h -1 The reaction results are shown in Table 3.
[0082] Comparative Example 1
[0083] Reduction and reaction were carried out in the same manner as in Example 1, except that catalyst A was used and the reaction temperature was 200° C. The results are shown in Table 3.
[0084] Example 2
[0085] Reduction and reaction were carried out in the same manner as in Example 1, except that catalyst F was used and the reaction temperature was 190°C. The results are shown in Table 3.
[0086] Comparative Example 2
[0087] Reduction and reaction were carried out in the same manner as in Example 1, except that catalyst E was used and the reaction temperature was 220°C. The results are shown in Table 3.
[0088] Example 3
[0089] Reduction and reaction were carried out in the same manner as in Example 1, except that catalyst D was used and the reaction temperature was 220°C. The results are shown in Table 3.
[0090] Comparative Example 3
[0091] Reduction and reaction were carried out in the same manner as in Example 1, except that the catalyst was C and the reaction temperature was 230°C. The results are shown in Table 3.
[0092] Example 4
[0093] Reduction and reaction were carried out in the same manner as in Example 1, except that the catalyst B1 was used and the reaction temperature was 170°C. The results are shown in Table 3.
[0094] Table 3 Catalyst evaluation results
[0095]
[0096] As can be seen from Table 3, Examples 1-4 and Comparative Examples 1-3 demonstrate that the catalysts of the present application achieve higher feedstock conversion rates at lower temperatures compared to catalysts without the addition of rhenium compounds, thereby achieving the goal of increasing the selectivity and yield of 1,4-butanediol. Furthermore, analysis of Examples 1-4 demonstrates that the catalysts of the present application can achieve the technical benefits of high conversion rates, high selectivity, and high yield of 1,4-butanediol at higher space velocities.
[0097] Unless otherwise defined, the terms used in the present invention have the same meanings as those commonly understood by those skilled in the art.
[0098] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above-mentioned embodiments, but is only limited by the claims.
Claims
1. A maleic anhydride hydrogenation catalyst, It is characterized in that The catalyst is cRe 2 O 7 / CuM1 a M2 b O x , Wherein, M1 and M2 each independently represent one or more of Al, Ti, Zr, Zn, K, Na, Ca, Mn, Mg, B, Se, Sb, P, C, Sn, Co, Fe, Ni, V, Cr, Mo, W, Si, Pd, Pt, Ag, Ru, Ga, In, Y, and rare earth metals; Preferably, M1 and M2 each independently represent Al, Ti, Zr, Zn, Mn, Co, Fe, Ni, La or Ce; Further preferably, M1 and M2 each independently represent Zr, Zn, Mn, Al or Fe; Still further preferably, M1 and M2 each independently represent Zr, Mn or Al; a is selected from 0-4; b is selected from 0-4; x is the number of oxygen atoms that satisfy the valence state of each metal atom; c is 0.01wt%-40.0wt%.
2. The catalyst according to claim 1, It is characterized in that c is 0.01 wt% to 10.0 wt%, more preferably 0.1 wt% to 4.0 wt%.
3. The catalyst according to claim 1, It is characterized in that a and b are not 0 at the same time.
4. The catalyst according to claim 1, It is characterized in that The catalyst is reduced before use, and the reducing agent is a reducing gas, preferably H 2 and / or CO; the reduction conditions are: the reduction pressure is 1.0-6.0MPa, the reduction temperature is 250-300°C; the reduction gas flow rate is 50-200 ml / min / g catalyst.
5. A method for preparing the catalyst according to any one of claims 1 to 4, It is characterized in that The specific steps include: (1) Dissolve or disperse the metal Cu, M1, and M2 compounds in water, add a precipitant, adjust the pH until the precipitation is complete, age, filter, collect the precipitate, dry, and calcine to obtain the composite oxide CuM1 a M2 b O x ; (2) The composite oxide CuM1 prepared in step (1) a M2 b O x Add Re 2 O 7 acetone solution, impregnated and dried to obtain the catalyst cRe 2 O 7 / CuM1 a M2 b O x .
6. A method for preparing the catalyst according to any one of claims 1 to 4, It is characterized in that The specific steps include: (a) dissolving or dispersing a compound of metal Cu, M1, and M2 in water, adding a precipitant, adjusting the pH until precipitation is complete, aging, filtering, collecting the precipitate, drying, and calcining to obtain a composite oxide CuM1 a M2 b O x ; (b) the composite oxide CuM1 prepared in step (a) a M2 b O x Add HReO 4 The aqueous solution is impregnated, dried and calcined to obtain the catalyst cRe 2 O 7 / CuM1 a M2 b O x .
7. The preparation method according to claim 5 or 6, It is characterized in that The metal compounds of Cu, M1 and M2 are soluble salts or oxides of Cu, M1 and M2; preferably nitrates or hydrochlorides; more preferably nitrates.
8. Use of the catalyst according to any one of claims 1 to 4 or the catalyst prepared by the preparation method according to any one of claims 5 to 7 in the preparation of 1,4-butanediol by hydrogenation of maleic anhydride.
9. The use according to claim 8, It is characterized in that The reaction temperature of the hydrogenation reaction is 140-280°C, preferably 140-220°C, more preferably 160-190°C, and the reaction pressure is 1.0-10.0Mpa; preferably 1.0-7.0Mpa; the molar ratio of hydrogen to raw material is (60-400):1, preferably (100-250):
1.
10. The use according to claim 8, It is characterized in that The molar ratio of the raw material maleic anhydride to the solvent is 0.1-5.0:
1.
11. The use according to claim 8, It is characterized in that The feed liquid hourly space velocity of raw material maleic anhydride is 0.1-1.0h -1 , preferably 0.1-0.6h -1 , more preferably 0.1-0.2h -1 , more preferably 0.1-0.14h -1 .