RuOx and sulfate radical co-modified CeO2 catalyst for catalytic combustion of 1, 2-dichloroethane as well as preparation method and application of RuOx and sulfate radical co-modified CeO2 catalyst

The Ru-CeO2-Sx catalyst prepared by co-precipitation method solved the problem of over-oxidation and decreased activity of the catalyst in catalytic combustion of 1,2-dichloroethane through sulfate modification, and achieved high activity and stability of the catalyst , avoiding the generation of polychlorinated by-products, achieving complete oxidation of 1,2-dichloroethane and meeting standard emissions.

CN119056469APending Publication Date: 2024-12-03EAST CHINA UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411395215.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing catalysts have excessive redox capabilities during the catalytic combustion of 1,2-dichloroethane, which leads to the generation of polychlorinated by-products, and surface acid modification leads to a decrease in catalyst activity, which cannot effectively inhibit the generation of incomplete oxidation by-products.

Method used

The Ru-CeO2-Sx catalyst was prepared by co-precipitation method. By introducing sulfate modification, a highly dispersed Ru and sulfate were formed in the CeO2 lattice semi-embedded state, exposing the active sites, enhancing the oxidation performance of the catalyst and introducing Browns A special acidic site to avoid the formation of polychlorinated by-products.

Benefits of technology

It significantly improves the activity, selectivity and stability of the catalyst, avoids the generation of polychlorinated by-products, achieves complete oxidation of 1,2-dichloroethane, meets the standard emissions, and realizes the chlorinated side at a lower reaction temperature. Effective removal of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a RuOx and sulfate radical co-modified CeO2 catalyst for catalytic combustion of 1, 2-dichloroethane as well as a preparation method and application of the RuOx and sulfate radical co-modified CeO2 catalyst. The Ru-CeO2-Sx catalyst is prepared from the following components in percentage by weight: 2.5 percent of Ru, 94.36 to 97.5 percent of CeO and 0 to 3.14 percent of Sx. The catalyst provided by the invention can completely oxidize 1, 2-dichloroethane into hydrogen chloride or chlorine, carbon dioxide and water at a lower reaction temperature, and then the hydrogen chloride or chlorine, carbon dioxide and water are absorbed by alkali liquor, so that standard emission of 1, 2-dichloroethane waste gas is realized, polychlorinated by-products with higher toxicity are not generated, and secondary pollution is avoided. 1000 ppm of 1, 2-dichloroethane can be completely eliminated at the temperature of 280 DEG C, and the conversion rate is kept stable in continuous 60 hours under the water-accompanying condition. The Ru-CeO2-Sx catalyst is prepared through a coprecipitation method, the activity, selectivity and stability of the catalyst can be remarkably improved, meanwhile, the preparation method is simple and easy to implement, and industrialization is easy to achieve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to RuO for catalytic combustion of 1,2-dichloroethane x and sulfate co-modified CeO2 catalyst and its preparation method and application, specifically, Ru-CeO2-S is prepared by co-precipitation method x Catalyst, belongs to the field of air pollution control. Background Art

[0002] Chlorinated volatile organic compounds (CVOCs) are important intermediates in industrial processes. Factories will inevitably release these compounds, causing serious harm to human health. At present, my country has formulated strict standards for the emission of air pollutants. For example, the "Emission Standards for Pollutants from Caustic Soda and Polyvinyl Chloride Industries" (GB 15581-2016) clearly stipulates that the emission concentration limit of vinyl chloride (VC) is 10 mg / m 3 The emission concentration limit of dichloroethane (DCE) is 5 mg / m 3 .

[0003] At present, noble metal catalysts, transition metal catalysts and rare earth catalysts have been mainly developed. Among all catalysts, noble metal catalysts are the most widely used in industrial applications. Ruthenium-based catalysts have been widely studied because of their excellent durability by effectively removing inorganic chlorine species. As reported in the literature (Appl. Catal. B-environ., 2013,129: 580-588), Ru / CeO2 catalysts have good activity for the catalytic oxidation of CVOCs. However, due to the lack of acidic sites, especially Bronsted acidic sites, and excessive redox ability, the generation of a large number of polychlorinated byproducts is inevitable. Surface acid modification is considered to be an ideal strategy to inhibit polychlorinated byproducts, especially for ruthenium-based catalysts. However, acidic surface modification inevitably leads to a decrease in the redox ability of the catalyst and the encapsulation of metal active sites, resulting in the production of incompletely oxidized byproducts during the catalytic combustion of CVOCs.

[0004] Although the various catalysts mentioned in the literature have their own advantages, there are still some inevitable problems. On the one hand, excessive redox ability during catalytic combustion is prone to produce polychlorinated byproducts, leading to secondary pollution; on the other hand, surface acid modification will lead to the deactivation of the active center of the catalyst, thereby reducing its activity and producing incomplete oxidation byproducts. Therefore, the development of catalysts with balanced redox ability and acidity has great practical application prospects. Summary of the invention

[0005] The object of the present invention is to provide a Ru-based catalyst for catalytic combustion reaction of 1,2-dichloroethane and a preparation method thereof, so as to overcome the shortcomings of existing catalysts.

[0006] The Ru-CeO2-S for catalytic combustion reaction of 1,2-dichloroethane of the present invention x The composition and weight percentage content of the catalyst are: Ru 2.5% CeO2 94.36~97.5% S x 0~3.14% The Ru-CeO2-S x The molar ratio of cerium sulfide in the catalyst is 0 to 0.3.

[0007] The Ru-CeO2-S for catalytic combustion reaction of 1,2-dichloroethane of the present invention x The catalyst is prepared by a co-precipitation method, which specifically includes the following steps: dissolving cerium nitrate in deionized water, then adding the required different ruthenium precursors and sulfate precursor solutions, stirring for 15 minutes to 2 hours, adjusting the pH value of the mixed solution to 8 to 10 with ammonia water, allowing it to be completely precipitated and aged at room temperature for 4 to 12 hours, then centrifuging the precipitate several times with water and ethanol, drying at 80 to 120°C for 8 to 12 hours, and then calcining at 400°C for 2 to 6 hours.

[0008] The Ru-CeO2-S x The catalyst is used in the catalytic combustion reaction of 1,2-dichloroethane. The catalytic reaction conditions are: the concentration of 1,2-dichloroethane is 1000 ppm, the concentration of water is 0% to 5%, and the reaction space velocity is 30000 mL·g -1 ·h -1 .

[0009] The significant advantage of the preparation method of the catalyst of the present invention is that Ru and sulfate are co-introduced into the CeO2 lattice by a simple co-precipitation method to prepare Ru-CeO2-S x When the catalyst is modified with low-content sulfate species, the Ru species is highly dispersed and partially exposed on the surface of the catalyst in a semi-embedded state, so that there is a strong interaction between Ru and sulfate species and CeO2, exposing more exposed Ce 3+ / 4+ The active sites such as oxygen vacancies make the catalyst have good activity and stability.

[0010] The significant advantage of the preparation method of the catalyst of the present invention is that the modification of sulfate species generates a new C-Cl bond breaking path, which enhances the oxidation performance of the catalyst and introduces Bronsted acid sites, which is beneficial to the removal of chlorine species, so that chlorination by-products are greatly suppressed and the selectivity of the catalyst is greatly improved.

[0011] One of the significant advantages of the catalyst of the present invention is that it does not generate more toxic polychlorinated by-products, avoids secondary pollution, and can completely oxidize 1,2-dichloroethane into hydrogen chloride or chlorine, carbon dioxide and water at a relatively low reaction temperature, and then absorbs them with alkaline solution to achieve standard emission of 1,2-dichloroethane waste gas.

[0012] The second significant advantage of the catalyst of the present invention is that the Ru-CeO2-S x The catalyst can significantly improve the activity, selectivity and stability of the catalyst, and the preparation method is simple and easy to implement industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The S content of 2.5 wt.% Ru-CeO2-S x The influence of catalyst on the catalytic activity of 1,2-dichloroethane; Figure 2 Sequential introduction of Ru and S species for 2.5 wt.% Ru-CeO2-S 0.05 The influence of catalyst on the catalytic activity of 1,2-dichloroethane; Figure 3 Precursor for Ru to 2.5 wt.% Ru-CeO2-S 0.05 The influence of catalyst on the catalytic activity of 1,2-dichloroethane; Figure 4 As a sulfate precursor for 2.5 wt.% Ru-CeO2-S 0.05 The influence of catalyst on the catalytic activity of 1,2-dichloroethane; Figure 5 2.5 wt.% Ru-CeO2-S 0.05 60-hour stability of the catalyst in the catalytic combustion of 1,2-dichloroethane. DETAILED DESCRIPTION

[0014] The present invention will be described in detail below with reference to specific embodiments, but this does not limit the protection scope of the present invention.

[0015] Comparative Example Preparation of CeO2 support: 2.523 g Ce(NO3)2·6H2O was calcined at 500 °C for 4 hours to obtain CeO2 support.

[0016] Preparation of 2.5 wt.% Ru / CeO2 catalyst: 1 g CeO2 carrier and 1.47 g Ru(NO)(NO3)3 aqueous solution (Ru content is 1.7 wt.%) were dispersed in 50 mL deionized water, stirred at room temperature for 12 hours, and excess water was removed by rotary evaporation at 50 °C. The catalyst was dried at 80 °C for 12 hours and calcined at 400 °C for 4 hours to obtain 2.5 wt.% Ru / CeO2 catalyst.

[0017] 2.5 wt.% S 0.05 / Ru / CeO2 and 2.5 wt.% S 0.05 Preparation of Ru / CeO2 catalyst: 1 g of Ru / CeO2 catalyst and 0.29 mL of 1 mol / L H2SO4 were dispersed in 50 mL of deionized water and stirred at room temperature for 12 h. Excess water was removed by rotary evaporation at 50 °C and dried at 80 °C for 12 h. The catalyst was calcined at 400 °C for 4 h. The catalyst was labeled as 2.5 wt.% S 0.05 / Ru / CeO2. 2.5 wt.% S 0.05 / Ru-CeO2 catalyst.

[0018] 2.5 wt.% Ru / S 0.05 Preparation of CeO2 / CeO2 catalyst: 1 g CeO2 support and 0.29 mL 1 mol / L H2SO4 were dispersed in 50 mL deionized water and stirred at room temperature for 12 h. Excess water was removed by rotary evaporation at 50 °C and dried at 80 °C for 12 h. The catalyst was calcined at 400 °C for 4 h and labeled as S 0.05 / CeO2 catalyst. Then, 1 gS 0.05 / CeO2 catalyst and 1.47 g Ru(NO)(NO3)3 aqueous solution (Ru content 1.7 wt.%) were dispersed in 50 mL deionized water and stirred at room temperature for 12 h. Excess water was removed by rotary evaporation at 50 °C and dried at 80 °C for 12 h. The catalyst was calcined at 400 °C for 4 h to obtain 2.5 wt.% Ru / S 0.05 / CeO2 catalyst.

[0019] 2.5 wt.% Ru / CeO2-S 0.05Preparation of catalyst: 2.523 g Ce(NO3)2·6H2O and 0.29 mL 1 mol / L H2SO4 were dissolved and stirred for 15 minutes, NH3·H2O solution (28 wt.%) was added dropwise, and the pH value was adjusted to 10 to allow complete precipitation. After aging for 4 hours, it was centrifuged with water and ethanol. It was dried at 80 °C for 12 hours and calcined at 400 °C for 4 hours. The catalyst was labeled as CeO2-S 0.05 catalyst, and then 1 g CeO2-S 0.05 and 1.47 g Ru(NO)(NO3)3 aqueous solution (Ru content 1.7 wt.%) were dispersed in 50 mL deionized water and stirred at room temperature for 12 h. Excess water was removed by rotary evaporation at 50 °C and dried at 80 °C for 12 h. The catalyst was calcined at 400 °C for 4 h to obtain 2.5 wt.% Ru / CeO2-S 0.05 catalyst.

[0020] 2.5 wt.% Ru-S 0.05 Preparation of / CeO2 catalyst: 1 g CeO2 carrier, 1.47 g Ru(NO)(NO3)3 aqueous solution (Ru content 1.7wt.%) and 0.29 mL 1 mol / L H2SO4 were dispersed in 50 mL deionized water, stirred at room temperature for 12 hours, and excess water was removed by rotary evaporation at 50 °C. Dry at 80 °C for 12 hours and calcine the catalyst at 400 °C for 4 hours. The catalyst with 2.5 wt.% Ru-S 0.05 / CeO2 catalyst. Example

[0021] 2.5 wt.% Ru-CeO2-S 0.05 Preparation of catalyst: 10.092 g Ce(NO3)2·6H2O was dissolved in 200 mL deionized water, and then 5.88 g Ru(NO)(NO3)3 aqueous solution (Ru content of 1.7 wt.%) and 1.16 mL H2SO4 (1 mol / L) solution were added. After stirring for 15 minutes, the pH value of the mixed solution was adjusted to 10 using NH3·H2O solution (28 wt.%), which was completely precipitated and aged at room temperature for 4 hours. The precipitate was centrifuged several times with water and ethanol, dried at 80 °C for 12 hours, and then calcined at 400 °C for 4 hours. The obtained catalyst was labeled as 2.5 wt.% Ru-CeO2-S 0.05 catalyst (where 0.05 is the molar ratio of S / Ce).

[0022] The catalytic performance evaluation conditions are as follows: the catalytic oxidation activity of CVOCs was tested in a fixed bed reactor. 240 mg of catalyst (40-60 mesh) was placed at the bottom and diluted with the same amount of quartz sand. The flow rate of dry air was controlled at 120 mL min -1 , corresponding to 30000 mL·g -1 ·h -1 The weight hourly space velocity was 1,2-dichloroethane. The concentration of 1,2-dichloroethane was 1000 ppm. During the test experiment, the reactor temperature was heated from 100 °C to 500 °C and maintained at each sampling temperature for 30 minutes. The composition of the tail gas was analyzed by an online gas chromatograph with a flame ionization detector.

[0023] Change Ru-CeO2-S x The molar ratios of sulfur and cerium in the catalyst were 0, 0.05, 0.1 and 0.3, respectively. 2.5 wt.% Ru-CeO2-S x The other preparation processes of the catalyst were the same as those of 2.5 wt.% Ru-CeO2-S 0.05 The catalyst is the same.

[0024] Effect of S content on the performance of 2.5 wt.% Ru-CeO2-S x The influence of catalyst on the catalytic activity of 1,2-dichloroethane Figure 1 shown. Example

[0025] Change 2.5 wt.% Ru-CeO2-S 0.05 The preparation process of the catalyst with different introduction order of Ru and S species is a comparative example, and the performance evaluation conditions are the same as those in Example 1.

[0026] Effect of the order of introduction of Ru and S species on the catalytic activity of 1,2-dichloroethane Figure 2 shown. Example

[0027] The Ru precursor was changed to RuCl3 aqueous solution (Ru content was 1.7 wt.%), 2.5 wt.% RuCl-CeO2-S 0.05 The preparation process and performance evaluation conditions of the catalyst are the same as those in Example 1.

[0028] Ru precursor for 2.5 wt.% Ru-CeO2-S x The influence of catalyst on the catalytic activity of 1,2-dichloroethane Figure 3 shown. Example

[0029] Changing the sulfate precursor to ammonium sulfate and sodium sulfate, ammonium sulfate (2.5 wt.% Ru-CeO2-AS 0.05 ) and sodium sulfate (2.5 wt.% Ru-CeO2-SS 0.05 ) The preparation process and performance evaluation conditions of the catalyst are the same as those in Example 1.

[0030] Sulfate precursors for 2.5 wt.% Ru-CeO2-S x The influence of catalyst on the catalytic activity of 1,2-dichloroethane Figure 4 shown. Example

[0031] 0.24 g of 2.5 wt.% Ru-CeO2-S prepared in Example 1 was added 0.05 The catalyst was placed in a quartz tube fixed bed reactor, with air as the oxidant, 1,2-dichloroethane concentration of 1000 ppm, water concentration of 5%, and reaction space velocity of 30000 mL·g -1 ·h -1 The 1,2-dichloroethane catalytic combustion reaction was carried out for 60 hours at a reaction temperature of 280 °C to investigate the high temperature stability of the catalyst. The experimental results are as follows Figure 5 As shown. Figure 5 It can be seen that within a reaction time of 60 hours, the conversion rate of 1,2-dichloroethane is close to 100% and is stable. Therefore, the catalyst has excellent high-temperature stability.

Claims

1. RuO for catalytic combustion of 1,2-dichloroethane x and sulfate co-modified CeO2 catalyst, characterized in that, The composition and weight percentage content of the catalyst are: Ru 2.5% CeO2 94.36~97.5% S x 0~3.14%。 2. The Ru-CeO2-S for catalytic combustion reaction of 1,2-dichloroethane according to claim 1 x A catalyst, characterized in that Ru-CeO2-S x The molar ratio of cerium sulfide in the catalyst is 0 to 0.

3.

3. RuO for catalytic combustion of 1,2-dichloroethane according to claim 1 x A method for preparing a CeO2 catalyst co-modified with sulfate, characterized in that: The preparation method is a co-precipitation method, which specifically includes the following steps: dissolving cerium nitrate in deionized water, then adding the required different ruthenium precursors and sulfate precursor solutions, stirring for 15 minutes to 2 hours, using ammonia water to adjust the pH value of the mixed solution to 8 to 10, allowing it to be completely precipitated and aged at room temperature for 4 to 12 hours, then centrifuging the precipitate several times with water and ethanol, drying at 80 to 120°C for 8 to 12 hours, and then calcining at 400°C for 2 to 6 hours.

4. RuO for catalytic combustion of 1,2-dichloroethane according to claim 1 x The application of CeO2 catalyst co-modified with sulfate is characterized in that: The catalytic reaction conditions are: the concentration of 1,2-dichloroethane is 1000 ppm, the concentration of water is 0% to 5%, and the reaction space velocity is 30000 mL·g -1 ·h -1 .

Citation Information

Patent Citations

  • Catalyst for catalytic combustion of VOCs as well as preparation method and application thereof

    CN110479317A

  • Ru (at) CexZr1-xO2 catalyst for catalytic combustion of vinyl chloride, and preparation method and application of Ru (at) CexZr1-xO2 catalyst

    CN117138779A

  • Preparation method and application of activated material loaded PtRu-CeO2-based composite catalyst

    CN117753412A

  • Ammonia synthesis catalyst

    JP2021109130A