Photocatalytic composite material and preparation method thereof

A composite photocatalytic material with lanthanum and manganese doping enhances photocatalytic activity and stability, addressing high recombination rates and selectivity issues, achieving efficient degradation of organic pollutants under visible light.

CN119056498APending Publication Date: 2024-12-03INST OF WENZHOU ZHEJIANG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411263724.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing photocatalytic materials face high preparation costs, poor stability, high recombination rates of photogenerated carriers, low visible light utilization, and insufficient selectivity in degrading organic pollutants, particularly in wastewater treatment.

Method used

A composite material is prepared by mixing lanthanum salt, manganese salt, metal oxide, and a dispersant, followed by thermal reaction and polymer treatment, to enhance photocatalytic activity, stability, and selectivity, with a polymer shell for specific pollutant degradation.

Benefits of technology

The composite material exhibits high catalytic activity, low recombination rates, and prolonged service life, effectively degrading organic pollutants under visible light, particularly azo dyes, with improved selectivity and efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of photocatalysis, and particularly relates to a photocatalytic composite material and a preparation method thereof. The method comprises the following steps: 1) uniformly mixing an oxidizing agent, a lanthanum salt, a manganese salt, a metal oxide and a dispersing agent, and performing thermal reaction, cleaning, drying and grinding to obtain powder; (2) uniformly mixing an ester compound, an initiator, a chain transfer agent and a dispersing agent, introducing inert gas, bubbling, discharging air, and carrying out heat treatment, drying and pretreatment to obtain a polymer; and (3) uniformly mixing the powder, organic titanium and absolute ethyl alcohol to obtain a solution A, uniformly mixing a polymer, an acid solution and a dispersing agent to obtain a solution B, dropwise adding the solution A into the solution B, mixing at a high speed, standing, aging and drying to obtain the photocatalytic composite material. Within a visible light range, the photocatalytic composite material prepared by the invention has relatively high catalytic activity, low photon-generated carrier recombination rate, very excellent degradation rate on methyl orange dye and azo dye, high stability and prolonged service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalysis, and in particular relates to a photocatalytic composite material and a preparation method thereof. Background Art

[0002] With the development of pharmaceutical, textile, printing and dyeing industries, organic raw materials are used in large quantities, especially in the textile industry, paper industry, pharmaceutical industry, tanneries and process bleaching industry, and various persistent organic pollutants have been introduced into our natural water resources or wastewater regeneration systems. Among them, the pharmaceutical and dye production processes are complicated, especially the pharmaceutical industry involves more unit reactions, such as sulfonation reaction, nitration reaction, reduction reaction, diazo and coupling reaction, etc. These reactions are the main links in the production of acidic wastewater in the process of drug and dye production. Together with the unreacted raw materials and by-products, their existence increases the difficulty of enterprises in treating wastewater. Since most dyes are easy to remain, difficult to degrade, and highly toxic to organisms, the discharged wastewater has seriously endangered human health, so water pollution control is very critical.

[0003] At present, water pollution control methods include adsorption, filtration, flocculation, sedimentation, etc. Among them, the photocatalytic oxidation method can be carried out at room temperature and pressure. The degradation power mainly comes from solar energy, and the reaction is safe and controllable. The photocatalytic materials added in the photocatalytic oxidation method can effectively destroy organic pollutants in wastewater, and no secondary treatment is required. The photocatalytic materials can be reused, which reduces the cost of use. Therefore, it is expected to become an effective way to solve environmental and energy problems.

[0004] However, the preparation cost of precious metal nano-photocatalytic composite materials is high, and the metal active components are easy to peel off or aggregate, which is difficult to fix on the carrier, and its stability is poor, resulting in reduced photocatalytic efficiency. Traditional photocatalytic materials have a large band gap width and low visible light utilization rate. In photocatalytic materials that are active in the visible light range, the recombination rate of photogenerated carriers and holes is fast, which significantly reduces the photocatalytic efficiency. At the same time, commercially available photocatalytic materials have poor selective degradation effects on specific pollutants. In summary, it is urgent to develop a new type of photocatalytic material to solve the above problems. Summary of the invention

[0005] Based on the above content, in order to solve the problems of high preparation cost, wide band gap, high recombination rate of photogenerated carriers, poor activity of effective components, poor stability and insufficient selectivity of photocatalytic materials, the present invention proposes a composite material and a preparation method thereof.

[0006] The objects of the present invention are:

[0007] 1. Improve the efficiency of light energy utilization by photocatalytic composite materials;

[0008] 2. Reduce the recombination rate of photogenerated carriers in photocatalytic composite materials and enhance the catalytic activity of photocatalytic materials;

[0009] 3. Enhance the stability of photocatalytic composite materials and extend their service life;

[0010] 4. Realize the selective degradation of specific pollutants by photocatalytic composite materials.

[0011] To achieve the above objectives, the present invention adopts the following technical solutions.

[0012] A method for preparing a photocatalytic composite material,

[0013] The method comprises:

[0014] 1) mixing an oxidant, a lanthanum salt, a manganese salt, a metal oxide and a dispersant uniformly, and subjecting the mixture to a thermal reaction, washing, drying and grinding to obtain a powder;

[0015] 2) mixing an ester compound, an initiator, a chain transfer agent and a dispersant uniformly, introducing an inert gas to bubble out the air, and obtaining a polymer through heat treatment, drying and pretreatment;

[0016] 3) Mix the powder, organic titanium and anhydrous ethanol to obtain liquid A, mix the polymer, acid solution and dispersant to obtain liquid B, drop liquid A into liquid B and mix at high speed, and obtain the photocatalytic composite material after standing, aging and drying.

[0017] As a preference,

[0018] Step 1) The oxidant is potassium permanganate;

[0019] Step 1) the lanthanum salt is lanthanum nitrate, and its dosage is 0.2-0.25 g / g oxidant;

[0020] Step 1) the manganese salt is manganese nitrate, and the amount thereof is 0.05 to 0.15 g / g oxidant;

[0021] Step 1) The metal oxide is titanium dioxide, and its usage is 10.0-10.2 g / g oxidant.

[0022] As a preference,

[0023] Step 1) The thermal reaction is carried out at 90-95°C for 60-72 hours;

[0024] The grinding in step 1) is to grind the powder obtained by drying to a size of ≥200 mesh.

[0025] As a preference,

[0026] Step 2) the ester compound is (2-dimethylaminoethyl) methacrylate, and its dosage is 8-12 mL / g oxidant;

[0027] Step 2) the initiator is diphenyl disulfide, and the amount used is 0.03-0.06 mL / mL of ester compound;

[0028] Step 2) the chain transfer agent is N-(morpholine-4-thiocarbonyl)benzamide, and its dosage is 0.01-0.02 g / mL ester compound;

[0029] Step 2) The dispersant is ethanol, and its usage is 5-10mL / mL ester compound.

[0030] As a preference,

[0031] Step 2) the bubbling time is ≥ 15 min;

[0032] Step 2) The heat treatment is carried out at a constant temperature of 60-65° C. for 22-24 hours.

[0033] As a preference,

[0034] Step 2) The pretreatment process is:

[0035] The polymer is immersed in a NaOH solution with a concentration of 0.3-0.4 mol / L at a constant temperature of 30-35°C for 2.5-3 hours, and after washing, the polymer is protonated with a HCl solution with a concentration of 0.1-0.2 mol / L for 3-3.5 hours, and then washed and dried for later use;

[0036] The dosage of the NaOH solution is 10-20 mL / g polymer.

[0037] As a preference,

[0038] Step 3) the organic titanium is tetrabutyl titanate, and its dosage is 3-5 mL / g oxidant;

[0039] Step 3) The amount of anhydrous ethanol used is 5-10 mL / mL of organic titanium;

[0040] Step 3) The amount of the polymer used is 0.2-0.4 g / mL of organic titanium;

[0041] Step 3) the acid solution is glacial acetic acid, and its dosage is 1-1.5 mL / mL organic titanium;

[0042] Step 3) The dispersant is a mixture of anhydrous ethanol and tetrahydrofuran, which is prepared in a volume ratio of 1: (2-2.5) and a dosage of 3-5 mL / mL of organic titanium.

[0043] As a preference,

[0044] Step 3) The high-speed mixing process is:

[0045] Add liquid A drop by drop, and the solution gradually turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours;

[0046] Step 3) The standing aging time is 2 to 3 hours.

[0047] The present invention is based on MnO 2 It can promote the separation of photogenerated electrons and photogenerated holes. Through compounding and modification, it can improve the photocatalytic activity of titanium dioxide-based photocatalytic composite materials, reduce the recombination rate of photogenerated carriers, and expand the light absorption range to the visible light region. In the technical solution of the present invention, the amount of lanthanum salt used has a significant effect on the actual doping effect. 3+ The crystal structure after doping will cause the interplanar spacing to change, and the increase in interplanar spacing will lead to a decrease in the diffraction angle. However, when the amount of lanthanum salt is small, the interplanar spacing and diffraction angle of the composite material are not changed, indicating that La 3+ Doping did not produce corresponding new phases. With the increase of lanthanum salt dosage, La 3+ Entering the lattice, the lattice expands and TiO 2 The oxygen vacancies and lattice defects on the crystal surface increased significantly, which significantly improved the activity of the photocatalytic composite material. Since lanthanum has an unfilled 4f shell structure, it can make TiO 2 Lattice distortion occurs, resulting in lattice defects, which causes new intermediate energy levels to appear between the original conduction band and valence band energy levels, narrowing the bandgap, facilitating electron transitions and improving the degradation efficiency of the composite material for organic dyes. In this composite material system, lanthanum doping makes TiO 2 The valence band shifts, the bandgap width narrows, and the energy required for electron excitation in the valence band is reduced. After characterization, it was found that the absorption edge of the composite material was red-shifted, and the doped composite material was more easily excited by visible light. Since the generation of lattice defects becomes the capture center of photogenerated carriers, La 3+ The photogenerated electrons are consumed, effectively inhibiting the recombination of photogenerated electron-hole pairs, thereby efficiently degrading organic pollutants. 2 The change in phase causes a significant decrease in the performance of the composite material, which indicates that lanthanum doping does not produce an absolutely beneficial effect. Instead, an appropriate amount of lanthanum doping can effectively inhibit the recombination of photogenerated electron-hole pairs and improve the photocatalytic quantum yield.

[0048] The present invention adopts MnO 2 Strong absorption of the entire solar wavelength band effectively converts light energy into heat energy, which drives the surface lattice oxygen to escape, and then the lattice oxygen escape catalytic reaction occurs, oxidizing organic pollutants into inorganic substances. The oxygen vacancies generated by the lattice oxygen escape are filled with oxygen in the air, achieving cyclic catalysis. According to the research of technicians in this field, α-MnO2 ,δ-MnO 2 The catalytic activity is similar to that of γ-MnO 2 ,β-MnO 2 The catalytic activity is high. This is mainly because the different concentrations of lattice oxygen defects on the surface of the material significantly affect the escape energy of the surface lattice oxygen, which has a significant impact on the catalytic activity of the composite material. 2 The surface forms MnO with controllable valence and crystal form 2 The present invention adopts the hydrothermal oxidation-reduction method and limits the amount of materials used. After characterization, it was found that lanthanum oxide and manganese oxide mostly grow on anatase TiO 2 {101} crystal face family, La 2 O 3 Crystal embedded in TiO 2 , cryptomelane octahedral structural units appear locally.

[0049] According to research by those skilled in the art, small-sized photocatalytic materials often have a higher specific surface area, that is, more active sites are exposed to the environment, which is conducive to improving the contact rate between the photocatalytic material and the reactant, enhancing the photocatalytic reaction rate, and the small-sized photocatalytic material has a better dispersion effect in sewage. Therefore, in addition to doping ions to form structural doping, the present invention grinds the product to reduce the size of the particles. To a certain extent, the larger the specific surface area of ​​the composite material, the stronger the photocatalytic activity will be, and the better the degradation effect on organic pollutants will be.

[0050] The above-mentioned materials can induce oxidation of refractory compounds such as tetracycline. In order to further improve the selectivity of the material for the degradation of azo-containing organic pollutants, the present invention prepares a polymer shell that can quickly bind hydroxylated derivatives, phenolic compounds, aromatic amines, naphthoquinones, and organic acids. The polymer shell plays a role in quickly binding organic pollutants, not only providing free radicals to participate in the reaction, but also catalyzing the breaking of the bond between the carbon atom and the adjacent nitrogen atom, thereby improving the degradation efficiency. The present invention obtains a polymer with a narrow distribution and controllable relative molecular weight by adding a specific chain transfer agent and regulating its dosage. Affected by the introduction of a thiocarbonyl-containing chain transfer agent, the polymer isomerizes, the isomeric end groups and the thiocarbonyl groups are superimposed and absorbed, and π-π+ electron transitions occur in the system. In practical applications, visible light irradiation allows the photocatalytic composite material to quickly reach a photosteady state. The photocatalytic composite material can combine with hydroxylated derivatives or phenolic compounds through nucleophilic addition to form new carbon-oxygen bonds. Especially in acidic environments, the material has high activity; it can be converted into a Schiff base intermediate with aromatic amines, and the sulfur atom attacks the nitrogen atom of the aromatic amine to form a new carbon-nitrogen bond, releasing the carbonyl component, and usually further forms a thiourea derivative; the nucleophilic reaction of the electron-rich aromatic ring and carboxylic acid group, the catalytic effect of the synergistic core, can achieve the rapid conversion of pollutants containing aromatic rings or carboxylic acid groups. At the same time, the decomposition of the thiocarbonyl chain segment releases free radicals, which is beneficial to improve the efficiency of photocatalytic degradation.

[0051] Furthermore, the present invention composites powder and polymer, and the composite material has an excellent degradation rate in an acidic environment. In order to form a polymer shell outside the powder that can provide more active sites, the present invention pre-treats the polymer. With the extension of the alkali treatment time, the mechanical properties of the polymer are seriously lost; with the increase of the treatment temperature, the polymer is easier to swell, the contact area between the solution and the polymer increases, the movement rate of NaOH molecules increases, and the reaction rate with the polymer increases, resulting in a significant decrease in its mechanical properties. With the increase of concentration, the mechanical properties of the polymer decrease more significantly. Under certain treatment conditions, the etching effect of low-concentration NaOH solution on the polymer surface is poor; the roughness of the polymer surface increases with the increase of the concentration of NaOH solution; with the treatment of a higher concentration of NaOH solution, the fineness of the polymer is greatly reduced, resulting in severe erosion and breakage, and decomposition into a short-powdered powder. In order to avoid the degradation of mechanical properties caused by the excessive fineness of the polymer, the present invention mainly limits the concentration of the NaOH solution. After treatment, micro-gaps appear on the surface of the polymer, which is degraded by NaOH, the macromolecular chains are broken, and the surface is activated. Through experiments, it was found that when the pH value of sewage is in the range of 2.1 to 5.2, since the polymer is protonated and has a positive charge on the surface, it has a good adsorption effect on anionic acidic azo dyes.

[0052] Under the synergistic effect of light and photocatalytic materials, the present invention evaluates the degradation efficiency of organic dyes. The dye generates cavitation under the action of ultrasound. When the energy of the irradiated light is equal to or greater than the bandgap width of the semiconductor photocatalytic composite material, electron-hole pairs are formed inside the composite material, and the excited electrons jump to the surface of the material and generate holes (h + ), while the electrons and the adsorbed O 2 react to generate superoxide radicals (·O 2- ). At the same time, the photogenerated holes can react with the hydroxyl groups on the surface of the material to generate hydroxyl radicals (·OH). Superoxide radicals and hydroxyl radicals are the active components of the photocatalytic reaction, which can degrade and mineralize organic pollutants.

[0053] The beneficial effects of the present invention are as follows:

[0054] (1) In the visible light range, the photocatalytic composite material prepared by the present invention has high catalytic activity and low recombination rate of photogenerated carriers;

[0055] (2) The photocatalytic composite material prepared by the present invention has strong stability and prolonged service life;

[0056] (3) The photocatalytic composite material prepared by the present invention has high degradation efficiency for 20 mg / L methyl orange dye and also has excellent degradation efficiency for azo dyes. DETAILED DESCRIPTION

[0057] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0058] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0059] Example 1

[0060] A method for preparing a photocatalytic composite material, the method comprising:

[0061] 1) 1 g potassium permanganate, 0.2 g lanthanum nitrate, 0.5 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95° C. for 60 h, washed and dried, and the dried powder was ground into 300 mesh;

[0062] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, 0.1 g N-(morpholine-4-thiocarbonyl) benzamide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.3 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0063] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0064] The performance of the photocatalytic composite material prepared in this example was tested using the following method.

[0065] 1. Photocatalytic degradation of methyl orange (azo dye):

[0066] Prepare a 20mg / L methyl orange solution, weigh 80mg of the photocatalytic composite material and add it to 80mL of a 20mg / L methyl orange solution. Start magnetic stirring and dark adsorption for 30min, fully mix to achieve adsorption and desorption equilibrium between the photocatalytic composite material and the methyl orange solution, eliminate the effect of adsorption on the concentration of the target pollutant, and sample 5mL. Install a xenon lamp just above the beaker, turn on the 300W xenon lamp source, sample 5mL every 20min, centrifuge the suspension at high speed for 10min, take the supernatant and test the absorbance of the obtained supernatant. The supernatant obtained by centrifugation is measured by a UV-visible spectrophotometer to determine the absorbance A of the characteristic wavelength of methyl orange at 665nm (A0), and the corresponding degradation rate D is calculated by the formula D=(1-A / A0)×100%.

[0067] 2. Thermal catalytic degradation of benzene:

[0068] Using WFS-2015, take 0.08g of photocatalytic composite material and fill it into the quartz tube of the equipment. The inner diameter of the quartz tube is 16±0.05mm and the length is 600±0.05mm. Place the thermocouple on the inner side of the reactor and contact the photocatalytic composite bed. The fixed bed quartz tube reactor is located in the middle of a temperature-controllable and heat-insulating tubular furnace. The synthesized compressed air is passed into a bubbler filled with benzene to provide a driving force to form a gas with a concentration of the saturated vapor pressure of benzene. Then, the compressed air synthesized from another route is combined with the gas with the above-mentioned concentration of the saturated vapor pressure of benzene. By controlling the amount of gas introduced from the two routes, the concentration of benzene in the mixed gas is adjusted. The initial reactant concentration of benzene is adjusted to 2g / m 3 The total flow rate is 40 mL / min (space velocity SV = 48000 mL / (g·h)). The benzene-containing bubbler oil bath is heated at 260°C, and the tail gas after contact with the photocatalytic composite material is connected to the GC9560 gas chromatograph. The product after contact between benzene and the photocatalytic composite material is CO 2 and H 2 O, calculated benzene consumption conversion based on the reaction mass.

[0069] 3. Low temperature catalytic activity test:

[0070] 0.08 g of the photocatalytic composite material was uniformly coated on the surface of a quartz glass slide of 4 cm × 4 cm in size, and the slide was fixed to the bottom of the gas phase reactor. A thermocouple was used to measure the reaction temperature of the photocatalytic composite material. The gas phase reactor was placed in an ice water bath, and a xenon lamp was turned on to irradiate the photocatalytic composite material until the CO in the gas phase reactor 2 The concentration tends to be stable. 2 When the concentration is stable, 80 mL of 20 mg / L methyl orange solution is injected into the reactor. Based on test (1), the low temperature photocatalytic degradation rate is calculated.

[0071] The results are as follows.

[0072] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 94.8 90.2 88.4

[0073] The photocatalytic composite material in this example has an increased number of nuclei, a reduced grain size, and an increased specific surface area, showing excellent catalytic activity and selectivity. 2 Based on the material, the composite material of the present invention can degrade benzene at a relatively low temperature. According to the research of those skilled in the art, TiO 2The starting temperature of catalytic oxidation of benzene is above 340°C, while the degradation rate is lower than 35% (31.5%), indicating that its catalytic activity is low. Under low temperature environment, the photocatalytic degradation rate of the composite material decreases, but it still shows strong catalytic activity; after continuous circulation for 24 hours, the composite material still shows strong catalytic activity. It can be seen that the photocatalytic composite material in this example has excellent structural stability.

[0074] Example 2

[0075] A method for preparing a photocatalytic composite material, the method comprising:

[0076] 1) 1 g potassium permanganate, 0.23 g lanthanum nitrate, 0.5 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95° C. for 60 h, washed and dried, and the dried powder was ground into 300 mesh;

[0077] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, 0.1 g N-(morpholine-4-thiocarbonyl) benzamide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.3 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0078] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0079] The photocatalytic composite material prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0080] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 95.3 90.5 88.6

[0081] According to the results in the table, as the amount of lanthanum salt increases, La 3+ Entering the lattice, the lattice expands and TiO 2 The oxygen vacancies and lattice defects on the crystal surface increased significantly, which significantly improved the activity of the photocatalytic composite material. 2The valence band shifts and the bandgap width becomes narrower, which reduces the energy required for electron excitation in the valence band. This is not only beneficial to electron transition and improves the degradation efficiency of the composite material for organic dyes, but also effectively inhibits the recombination of photogenerated electron-hole pairs, thereby efficiently degrading organic pollutants. In a low temperature environment, this material maintains a good degradation effect, indicating that the material has excellent structural stability.

[0082] Example 3

[0083] A method for preparing a photocatalytic composite material, the method comprising:

[0084] 1) 1 g potassium permanganate, 0.25 g lanthanum nitrate, 0.5 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95° C. for 60 h, washed and dried, and the dried powder was ground into 300 mesh;

[0085] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, 0.1 g N-(morpholine-4-thiocarbonyl) benzamide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.3 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0086] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0087] The photocatalytic composite material prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0088] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 94.9 90.4 88.4

[0089] According to the results in the table, it is found that when the amount of lanthanum salt is large, TiO 2 The phase change caused a significant decrease in the performance of the composite material, which shows that lanthanum doping does not produce an absolutely beneficial effect.

[0090] In addition, under the synergistic effect of light and photocatalytic materials, the present invention evaluates the degradation efficiency of organic dyes. Through experiments, it is found that in the range of sewage pH value of 2.1 to 5.2, since the polymer is protonated and has a positive charge on the surface, it has a good adsorption effect on anionic acidic azo dyes. Under the same conditions, the lower the initial pH of the dye solution of the simulated wastewater, the better the degradation effect after treatment. Acidic conditions are more conducive to the bond breaking and degradation of methyl orange. The CN bond adjacent to azo has higher activity than the N=N bond, and breaks first. The CN bond is mainly attacked by oxidation.

[0091] Comparative Example 1

[0092] A method for preparing a photocatalytic composite material, the method comprising:

[0093] 1) 1 g potassium permanganate, 0.1 g lanthanum nitrate, 0.5 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95° C. for 60 h, washed and dried, and the dried powder was ground into 300 mesh;

[0094] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, 0.1 g N-(morpholine-4-thiocarbonyl) benzamide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.3 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0095] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0096] The photocatalytic composite material prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0097] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 87.1 74.3 76.5

[0098] Because of La 3+ The crystal structure after doping will cause the interplanar spacing to change, and the increase in interplanar spacing will lead to a decrease in the diffraction angle. However, when the amount of lanthanum salt is small, the interplanar spacing and diffraction angle of the composite material are not changed, indicating that La 3+Doping does not produce corresponding new phases. Combining the results in Examples 1 to 3 and Comparative Example 1, in the technical solution of the present invention, the amount of lanthanum salt used has a significant impact on the actual doping effect, and the appropriate lanthanum doping amount can effectively inhibit the recombination of photogenerated electron-hole pairs and improve the photocatalytic quantum yield.

[0099] Comparative Example 2

[0100] A method for preparing a photocatalytic composite material, the method comprising:

[0101] 1) 1 g potassium permanganate, 0.2 g lanthanum nitrate, 0.4 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95 ° C for 60 h, washed and dried, and the dried powder was ground into 300 mesh;

[0102] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, 0.1 g N-(morpholine-4-thiocarbonyl) benzamide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.3 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0103] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0104] The photocatalytic composite material prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0105] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 88.2 80.7 82.6

[0106] The present invention adopts MnO 2 The strong absorption of the entire solar wavelength effectively converts light energy into heat energy, which drives the surface lattice oxygen to escape, and then the lattice oxygen escape catalytic reaction occurs, oxidizing organic pollutants into inorganic substances. The oxygen vacancies generated by the lattice oxygen escape are filled with oxygen in the air, achieving cyclic catalysis. After characterization, the manganese oxide quantum dots on the surface of this composite material are β-MnO 2 According to research conducted by those skilled in the art, β-MnO 2Catalytic activity and α-MnO 2 ,δ-MnO 2 This is mainly because the different concentrations of lattice oxygen defects on the surface of the material significantly affect the escape energy of the surface lattice oxygen, which has a significant impact on the catalytic activity of the composite material. The photocatalytic degradation effect of the composite material in this example is poor.

[0107] Comparative Example 3

[0108] A method for preparing a photocatalytic composite material, the method comprising:

[0109] 1) 1 g potassium permanganate, 0.2 g lanthanum nitrate, 0.5 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95° C. for 60 h, washed and dried, and the dried powder was ground into 60 mesh;

[0110] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, 0.1 g N-(morpholine-4-thiocarbonyl) benzamide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.3 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0111] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0112] The photocatalytic composite material prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0113] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 83.9 77.0 76.9

[0114] According to research by those skilled in the art, small-sized photocatalytic materials often have a higher specific surface area, that is, more active sites are exposed to the environment, which is conducive to increasing the contact rate between the photocatalytic material and the reactants and enhancing the photocatalytic reaction rate. The composite material in this example has a smaller specific surface area, poorer photocatalytic activity, and significantly reduced degradation effect on organic pollutants.

[0115] Comparative Example 4

[0116] A method for preparing a photocatalytic composite material, the method comprising:

[0117] 1) 1 g potassium permanganate, 0.2 g lanthanum nitrate, 0.5 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95° C. for 60 h, washed and dried, and the dried powder was ground into 300 mesh;

[0118] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.3 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0119] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0120] The photocatalytic composite material prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0121] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 81.7 74.6 83.8

[0122] In this example, no chain transfer agent was added, and the obtained polymer shell had a wide distribution and a large relative molecular weight. In practical applications, the rate of reaching the photostable state was slow, and the rates of reactions such as nucleophilic addition of photocatalytic composite materials and attack on the nitrogen atom of aromatic amines were significantly reduced, that is, the rate of releasing free radicals was slow and the photocatalytic degradation efficiency was low.

[0123] Comparative Example 5

[0124] A method for preparing a photocatalytic composite material, the method comprising:

[0125] 1) 1 g potassium permanganate, 0.2 g lanthanum nitrate, 0.5 g manganese nitrate, 10 g titanium dioxide and 50 mL water were mixed evenly, kept at 95° C. for 60 h, washed and dried, and the dried powder was ground into 300 mesh;

[0126] 2) Mix 10 mL (2-dimethylaminoethyl) methacrylate, 0.3 mL diphenyl disulfide, 0.1 g N-(morpholine-4-thiocarbonyl) benzamide, and 50 mL ethanol, and pass N 2 The air was expelled by bubbling for 15 minutes, and the temperature was kept constant at 60°C for 24 hours. The dried polymer was immersed in a 0.8 mol / L NaOH solution, and 10 mL of NaOH solution was added per gram of polymer. The temperature was kept constant at 35°C for 2.5 hours. After washing, the polymer was protonated with a 0.1 mol / L HCl solution for 3.5 hours, and then washed and dried for use;

[0127] 3) Take powder, 3 mL of tetrabutyl titanate, and 15 mL of anhydrous ethanol and mix them evenly to obtain liquid A. Take 0.6 g of polymer, 4 mL of glacial acetic acid, 3 mL of anhydrous ethanol, and 7.5 mL of tetrahydrofuran and mix them evenly to obtain liquid B. Add liquid A drop by drop into liquid B, and the solution turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours, let it stand for 3 hours, and dry to obtain a photocatalytic composite material.

[0128] The photocatalytic composite material prepared in this example was subjected to the same performance test as in Example 1, and the results are as follows.

[0129] Photocatalytic degradation rate (%, room temperature) Benzene consumption conversion rate (%) Photocatalytic degradation rate (%, low temperature) 90.6 86.7 85.1

[0130] Under certain treatment conditions, this example used a relatively high concentration of NaOH solution to treat the polymer, which greatly reduced the fineness of the polymer, resulting in severe erosion, shedding, and breakage, and decomposition into a short-powdered state. The polymer was too fine, resulting in reduced mechanical properties. Compared with Example 2, the photocatalytic composite material in this example easily floated on the surface of the dye solution, and the photocatalytic degradation rate was lower within the same exposure time.

Claims

1. A method for preparing a photocatalytic composite material, characterized in that: The method comprises: 1) mixing an oxidant, a lanthanum salt, a manganese salt, a metal oxide and a dispersant uniformly, and subjecting the mixture to a thermal reaction, washing, drying and grinding to obtain a powder; 2) mixing an ester compound, an initiator, a chain transfer agent and a dispersant uniformly, introducing an inert gas to bubble out the air, and obtaining a polymer through heat treatment, drying and pretreatment; 3) Mix the powder, organic titanium and anhydrous ethanol to obtain liquid A, mix the polymer, acid solution and dispersant to obtain liquid B, drop liquid A into liquid B and mix at high speed, and obtain the photocatalytic composite material after standing, aging and drying.

2. The method for preparing a photocatalytic composite material according to claim 1, characterized in that: Step 1) The oxidant is potassium permanganate; Step 1) the lanthanum salt is lanthanum nitrate, and its dosage is 0.2-0.25 g / g oxidant; Step 1) the manganese salt is manganese nitrate, and the amount thereof is 0.05 to 0.15 g / g oxidant; Step 1) The metal oxide is titanium dioxide, and its usage is 10.0-10.2 g / g oxidant.

3. The method for preparing a photocatalytic composite material according to claim 1 or 2, characterized in that: Step 1) The thermal reaction is carried out at 90-95°C for 60-72 hours; The grinding in step 1) is to grind the powder obtained by drying to a size of ≥200 mesh.

4. The method for preparing a photocatalytic composite material according to claim 1, characterized in that: Step 2) the ester compound is (2-dimethylaminoethyl) methacrylate, and its dosage is 8-12 mL / g oxidant; Step 2) the initiator is diphenyl disulfide, and the amount used is 0.03-0.06 mL / mL of ester compound; Step 2) the chain transfer agent is N-(morpholine-4-thiocarbonyl)benzamide, and its dosage is 0.01-0.02 g / mL ester compound; Step 2) The dispersant is ethanol, and its usage is 5-10mL / mL ester compound.

5. The method for preparing a photocatalytic composite material according to claim 1 or 4, characterized in that: Step 2) the bubbling time is ≥ 15 min; Step 2) The heat treatment is carried out at a constant temperature of 60-65° C. for 22-24 hours.

6. The method for preparing a photocatalytic composite material according to claim 1, characterized in that: Step 2) The pretreatment process is: The polymer is immersed in a NaOH solution with a concentration of 0.3-0.4 mol / L at a constant temperature of 30-35°C for 2.5-3 hours, and after washing, the polymer is protonated with a HCl solution with a concentration of 0.1-0.2 mol / L for 3-3.5 hours, and then washed and dried for later use; The dosage of the NaOH solution is 10-20 mL / g polymer.

7. The method for preparing a photocatalytic composite material according to claim 1, characterized in that: Step 3) the organic titanium is tetrabutyl titanate, and its dosage is 3-5 mL / g oxidant; Step 3) The amount of anhydrous ethanol used is 5-10 mL / mL of organic titanium; Step 3) The amount of the polymer used is 0.2-0.4 g / mL of organic titanium; Step 3) the acid solution is glacial acetic acid, and its dosage is 1-1.5 mL / mL organic titanium; Step 3) The dispersant is a mixture of anhydrous ethanol and tetrahydrofuran, which is prepared in a volume ratio of 1: (2-2.5) and a dosage of 3-5 mL / mL of organic titanium.

8. The method for preparing a photocatalytic composite material according to claim 1 or 7, characterized in that: Step 3) The high-speed mixing process is: Add liquid A drop by drop, and the solution gradually turns light blue. After adding liquid A, keep mixing at high speed for 1 to 1.5 hours; Step 3) The standing aging time is 2 to 3 hours.

9. A photocatalytic composite material prepared by the method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of reduced graphene oxide / titanium dioxide double-shell hollow-sphere composite photocatalysis material

    CN109833862A

  • Surface modification of titanium oxide base light catalyzed material