Semiconductor device for improving coverage rate of metal step and preparation method thereof

By forming a slope structure on the metal steps using a tantalum nitride and aluminum-copper alloy layer modification, the method addresses poor insulating film uniformity, enhancing electrical insulation and preventing short circuits in microfluidic biochips.

CN119056507AInactive Publication Date: 2024-12-03SHANGHAI IND U TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187472.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Microfluidic biochips face issues with poor uniformity of the insulating film layer covering metal steps, particularly at the corner of the step sidewall, leading to potential short circuits and chip failure due to voltage breakdown.

Method used

A method involving the growth of a tantalum nitride layer, followed by an aluminum-copper alloy layer modification, wet etching to form a slope structure, deposition of a silicon nitride insulating layer, and finally a top metal layer to improve metal step coverage and uniformity, using a photophobic resist and specific etching solutions to reduce sidewall verticality.

Benefits of technology

The method enhances metal step coverage and uniformity, ensuring effective electrical insulation between upper and lower metal layers, preventing short circuits and improving chip performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056507A_ABST
    Figure CN119056507A_ABST
Patent Text Reader

Abstract

The invention discloses a semiconductor device for improving the coverage rate of metal steps and a preparation method thereof. The preparation method comprises the following steps: growing a tantalum nitride layer on the surface of a substrate; growing an aluminum-copper alloy layer on the surface of the tantalum nitride layer, and modifying the surface of the aluminum-copper alloy layer to obtain a sparse photoresist surface; coating photoresist on the surface of the sparse photoresist, and patterning the photoresist to form a photoresist layer; performing wet etching on the aluminum-copper alloy layer to form a slope structure with a narrow upper part and a wide lower part; depositing silicon nitride on the surface of the slope structure of the aluminum-copper alloy layer to serve as an insulating layer; and growing top-layer metal on the insulating layer, and photoetching the top-layer metal to form a metal pattern. According to the invention, the verticality of the side wall of the step is reduced to form a slope with a certain angle, so that the metal step is high in coverage, good in uniformity and high in stability after the DEP of the insulating medium is deposited, the upper and lower layers of metal are better electrically insulated, and a chip effectively works.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to a semiconductor device with improved metal step coverage and a preparation method thereof. Background Art

[0002] Microfluidic biochip is a microchip made by micromachining technology. It contains a tiny channel network and corresponding control components, which can perform precise fluid manipulation and has the advantages of fast, efficient, repeatable and low cost. With the continuous development of micromachining technology and material science, microfluidic chips are widely used in life science research, chemical analysis, laboratory diagnosis and personalized medicine.

[0003] Microfluidic biochips have high requirements for internal electrical insulation, and short circuits in internal circuits will directly affect product performance. Microfluidic biochips require that the internal insulating film have good insulation properties, and place high demands on the coverage and uniformity of the insulating film. Currently, in the preparation process of biochips, the sidewall verticality of the etching step is relatively large, and the insulating film layer formed on the step using the subsequent DEP process has poor uniformity in covering the metal step, especially at the corner of the step sidewall where the insulating film layer is thinner. Then a layer of metal is sputtered. In the thinner area of ​​the insulating layer, the upper and lower metal layers are prone to voltage breakdown, forming a short circuit, causing the chip to fail. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a semiconductor device with improved metal step coverage and a preparation method thereof, which reduces the verticality of the step sidewall and forms a slope structure with a certain angle, so that the insulating medium has high coverage, good uniformity and strong stability on the metal step after DEP deposition, thereby better electrically insulating the upper and lower layers of metal and enabling the chip to work effectively.

[0005] A technical solution adopted by the present invention is to provide a method for improving metal step coverage, comprising:

[0006] Step 1: growing a tantalum nitride layer on the substrate surface;

[0007] Step 2: growing an aluminum-copper alloy layer on the surface of the tantalum nitride layer, and modifying the surface of the aluminum-copper alloy layer to obtain a photophobic resist surface;

[0008] Step 3: coating a photoresist on the surface of the photophobic resist and patterning the photoresist to form a photoresist layer;

[0009] Step 4: wet-etching the aluminum-copper alloy layer to form a slope structure that is narrow at the top and wide at the bottom;

[0010] Step 5: depositing silicon nitride as an insulating layer on the slope structure surface of the aluminum-copper alloy layer;

[0011] Step six: growing a top metal layer on the insulating layer, and photolithographically etching the top metal layer to form a metal pattern.

[0012] In the step 2, the surface of the aluminum-copper alloy layer is modified: the surface of the aluminum-copper alloy layer is pretreated with a tetramethylammonium hydroxide solution, thereby modifying the surface of the aluminum-copper alloy layer to obtain a photorepellent surface, thereby reducing the adhesion between the photoresist and the surface of the aluminum-copper alloy layer.

[0013] In the step 2, the pretreatment time is 1 to 3 minutes.

[0014] In the step 3, when the photoresist is patterned, no hard baking is performed. Omitting the hard baking step can reduce the adhesion between the aluminum-copper alloy layer and the photoresist, increase the corrosion rate of the aluminum-copper alloy, and facilitate the formation of a slope structure of the aluminum-copper alloy layer that is narrow at the top and wide at the bottom.

[0015] In step 4, the angle of the slope structure is 35° to 85°.

[0016] In step 4, the solution used for wet etching is a mixed solution of phosphoric acid, nitric acid and acetic acid, and the volume ratio of the mixed solution is phosphoric acid: nitric acid: acetic acid = (1-60): (1-3): (1-3). By adjusting the volume ratio of phosphoric acid, nitric acid and acetic acid in the mixed solution, aluminum-copper slope structures with different angles are prepared.

[0017] The temperature of the wet etching solution is 30-50°C.

[0018] In the step 3, the thickness of the photoresist layer is 1-5 um. By adjusting the thickness of the photoresist layer, aluminum-copper slope structures with different angles are prepared.

[0019] In the step 4, the over-corrosion amount of the wet etching is 5% to 30%.

[0020] The present invention also provides a semiconductor device with improved metal step coverage, wherein the semiconductor device is prepared using a method for improving metal step coverage as described in any one of the above technical solutions.

[0021] The beneficial effects of the present invention are as follows: a semiconductor device with improved metal step coverage and a preparation method thereof of the present invention reduces the verticality of the step sidewall to form a metal step slope of a certain angle, so that the insulating medium has high coverage, good uniformity and strong stability on the metal step after DEP deposition, thereby better electrically insulating the upper and lower metal layers and allowing the chip to work effectively. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 is a flow chart of a method for improving metal step coverage of the present invention;

[0024] Figure 2 is a schematic diagram of the structure after processing in step 1 in Example 1 of the present invention;

[0025] Figure 3 It is a schematic diagram of the structure after processing in step 2 and step 3 in Example 1 of the present invention;

[0026] Figure 4 It is a schematic diagram of the structure after processing in step 4 in Example 1 of the present invention;

[0027] Figure 5 is a schematic diagram of the structure after processing in step 5 in Example 1 of the present invention;

[0028] Figure 6 is a schematic diagram of the structure after processing in step six in Example 1 of the present invention;

[0029] Figure 7 This is a schematic diagram of the slope structure of the aluminum-copper alloy layer in Example 1 of the present invention;

[0030] Figure 8 This is a schematic diagram of the slope structure of the aluminum-copper alloy layer in Example 2 of the present invention;

[0031] Fig. 9 This is a schematic diagram of the slope structure of the aluminum-copper alloy layer in Example 3 of the present invention;

[0032] Fig.10 Schematic diagram of the slope structure of the aluminum-copper alloy layer in Example 4 of the present invention.

[0033] 1. Titanium nitride layer (TIN); 2. Silicon nitride layer (SIN); 3. Photoresist layer (PR); 4. Aluminum-copper alloy layer (ALCU); 5. Tantalum nitride layer (TAN); 6. Substrate. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Examples of these preferred embodiments are illustrated in the accompanying drawings. The embodiments of the present invention shown in the accompanying drawings and described according to the accompanying drawings are merely exemplary, and the present invention is not limited to these embodiments.

[0035] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the solutions according to the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.

[0036] Example 1

[0037] See also Figure 1 The present invention provides a method for improving metal step coverage, comprising the following steps:

[0038] Step 1: If Figure 2 As shown, a tantalum nitride layer 5 is sputtered on the surface of a substrate 6. In this embodiment, the thickness of the substrate 6 is 725 um.

[0039] Step 2: sputtering an aluminum-copper alloy layer 4 on the surface of the tantalum nitride layer 5 to modify the surface of the aluminum-copper alloy layer 4. Specifically, the surface of the aluminum-copper alloy layer 4 is pretreated with a tetramethylammonium hydroxide (TMAH) solution to modify the surface of the aluminum-copper alloy layer 4 and obtain a photophobic resist surface. The pretreatment time is 1 to 3 minutes.

[0040] Step 3: Apply photoresist to the photoresist film, and pattern the photoresist to form a photoresist layer 3. Specifically, a photoresist with a thickness of 1 to 5 um is spin-coated on the surface of the pretreated aluminum-copper alloy layer 4, and a mask is placed on the photoresist and exposed to light, so that the desired pattern is imprinted on the photoresist film. In this embodiment, the thickness of the spin-coated photoresist is 4 um. After the photoresist is developed, the hard baking step is omitted, so that the adhesion between the photoresist and the aluminum-copper alloy layer 4 is reduced. The photoresist is patterned by photolithography to form a photoresist layer (PR) 3 on the surface of the aluminum-copper alloy layer 4, see Figure 3 .

[0041] Step 4: If Figure 4As shown, the aluminum-copper alloy layer 4 is wet-etched to form a slope structure that is narrow at the top and wide at the bottom; and the photoresist layer 3 is removed. Furthermore, during the wet etching process, the wet etching solution used is a mixed solution of phosphoric acid, nitric acid and acetic acid, and the volume ratio of the mixed solution is phosphoric acid: nitric acid: acetic acid = (1-60): (1-3): (1-3). In this embodiment, the volume ratio of the mixed solution is phosphoric acid: nitric acid: acetic acid = 30:2:1. The temperature of the wet etching solution is 30-50°C. The over-etching amount (OE) of the wet etching is 5%-30%. In this embodiment, the over-etching amount (OE) of the wet etching is 5%, and the angle α of the aluminum-copper alloy slope structure formed is 40°, see Figure 7 .

[0042] In the process of forming the aluminum-copper alloy slope structure, the adhesion between the photoresist layer 3 and the aluminum-copper alloy layer 4, and between the aluminum-copper alloy layer 4 and the tantalum nitride layer 5 is crucial. In the lateral etching process of wet etching, when the adhesion between the photoresist layer 3 and the aluminum-copper alloy layer 4 is slightly poor, and the adhesion between the aluminum-copper alloy layer 4 and the tantalum nitride layer 5 is strong, due to the difference in adhesion between the upper and lower layer interfaces, it is easier to form an aluminum-copper alloy slope structure with a certain angle. Therefore, the use of TMAH solution in step 2 to pretreat the surface of the aluminum-copper alloy layer 4, and the skipping of the hard baking step in step 3, are all to reduce the adhesion between the aluminum-copper alloy layer 4 and the photoresist, increase the etching rate, and form a slope structure of the aluminum-copper alloy layer 4 that is narrow at the top and wide at the bottom.

[0043] Step 5: If Figure 5 As shown, a silicon nitride insulating layer 2 is deposited by DEP on the slope surface of the aluminum-copper alloy layer 4;

[0044] Step 6: If Figure 6 As shown, a top metal titanium nitride layer 1 is sputtered on the silicon nitride insulating layer 2, and the titanium nitride layer 1 is photoetched to form a metal pattern.

[0045] Example 2

[0046] In this embodiment, except that the thickness of the photoresist in step 3 and the angle of the aluminum-copper alloy slope structure obtained are different from those in embodiment 1, the other aspects are exactly the same as those in embodiment 1. In embodiment 1, the thickness of the photoresist spun on is 4 um, and the angle of the copper-aluminum alloy slope obtained is 40°. In this embodiment, the thickness of the photoresist spun on in step 3 is 2.2 um, and the aluminum-copper alloy slope structure with an angle of 58° is finally obtained. Figure 8 The inventors found that when a 1-3 um thin glue is spin-coated, the AlCu slope angle is 45°-60°; when a 4-5 um thick glue is spin-coated, the AlCu slope is more gentle, with an angle of 35-45°, and the subsequent insulating layer has the best coverage and good insulation, and the effect of preventing the break down phenomenon is better.

[0047] Example 3

[0048] In this embodiment, except for the different ratio of the wet etching solution in step 4 from that in embodiment 1, the rest is exactly the same as embodiment 1. In embodiment 1, the volume ratio of the wet etching solution used is phosphoric acid: nitric acid: acetic acid = 30:2:1, and the obtained copper-aluminum alloy slope angle is 40°. In this embodiment, the volume ratio of the wet etching solution used is phosphoric acid: nitric acid: acetic acid = 1:2:1, and the aluminum-copper alloy slope structure with an angle of 35° is finally obtained, see Fig. 9 .

[0049] Example 4

[0050] In this embodiment, except for the over-corrosion amount (OE) of the wet etching in step 4 and the angle of the aluminum-copper alloy slope structure obtained, the other aspects are exactly the same as those of embodiment 1. In embodiment 1, the over-corrosion amount (OE) of the wet etching is 5%, and the angle of the copper-aluminum alloy slope obtained is 40°. In this embodiment, the over-corrosion amount (OE) of the wet etching is 20%, and the aluminum-copper alloy slope structure with an angle of 35° is finally obtained. Fig.10 .

[0051] In summary, by controlling the thickness of the spin-coated photoresist, the volume ratio of each solution in the wet etching solution used, and the over-corrosion amount of the wet etching within a certain range, an aluminum-copper alloy slope structure with an angle of 35° to 85° can be obtained. Specifically, the thickness of the spin-coated photoresist is 1 to 5 um, the volume ratio of each solution in the wet etching solution used is phosphoric acid: nitric acid: acetic acid = (1 to 60): (1 to 3): (1 to 3), and the over-corrosion amount of the wet etching is 5% to 30%.

[0052] The present invention also includes a semiconductor device with improved metal step coverage, characterized in that it is prepared using a method for improving metal step coverage as described in any one of the above technical solutions.

[0053] In addition, it should be noted that in this specification, "includes", "comprising" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprising a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0054] It should be understood that although this specification is described according to implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A method for improving metal step coverage, characterized in that: include: Step 1: growing a tantalum nitride layer on the substrate surface; Step 2: growing an aluminum-copper alloy layer on the surface of the tantalum nitride layer, and modifying the surface of the aluminum-copper alloy layer to obtain a photophobic resist surface; Step 3: coating a photoresist on the surface of the photophobic resist and patterning the photoresist to form a photoresist layer; Step 4: wet-etching the aluminum-copper alloy layer to form a slope structure that is narrow at the top and wide at the bottom; Step 5: depositing silicon nitride as an insulating layer on the slope structure surface of the aluminum-copper alloy layer; Step six: growing a top metal layer on the insulating layer, and photolithographically etching the top metal layer to form a metal pattern.

2. A method for improving metal step coverage according to claim 1, characterized in that: In the step 2, the surface of the aluminum-copper alloy layer is modified: the surface of the aluminum-copper alloy layer is pretreated by a tetramethylammonium hydroxide solution.

3. A method for improving metal step coverage according to claim 2, characterized in that: In the step 2, the pretreatment time is 1 to 3 minutes.

4. The method for improving metal step coverage according to claim 1, characterized in that: In the step three, when the photoresist is patterned, no hard baking process is performed.

5. The method for improving metal step coverage according to claim 1, characterized in that: In step 4, the angle of the slope structure is 35° to 85°.

6. The method for improving metal step coverage according to claim 1, characterized in that: In the step 4, the solution used for wet etching is a mixed solution of phosphoric acid, nitric acid and acetic acid, and the volume ratio of the mixed solution is phosphoric acid: nitric acid: acetic acid = (1-60): (1-3): (1-3).

7. The method for improving metal step coverage according to claim 1, characterized in that: The temperature of the wet etching solution is 30-50°C.

8. The method for improving metal step coverage according to claim 1, characterized in that: In the step three, the thickness of the photoresist layer is 1 to 5 um.

9. The method for improving metal step coverage according to claim 1, characterized in that: In the step 4, the over-corrosion amount of the wet etching is 5% to 30%.

10. A semiconductor device with improved metal step coverage, characterized in that: The metal step coverage is improved by using the method for improving the metal step coverage described in any one of claims 1 to 9.