Flotation method for improving fluorite recovery rate

By adjusting the ore feeding concentration and chemical dosage at each operation stage in the fluorite flotation process, the recovery rate of fluorite is improved, the problem of low fluorite recovery rate in the existing technology is solved, and more efficient fluorite resources are achieved. Recycling and cost reduction.

CN119056573AActive Publication Date: 2024-12-03CHINA MINMETALS CHANGSHA MINING RES INST

Patent Information

Application Number
CN202411169122.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The fluorite recovery rate in the existing fluorite flotation process is low, especially in the sweeping and selection stages, which leads to serious fluorite dropout, affecting the recovery rate. The existing improvement method is costly and effective. Not significant.

Method used

By intervening in the ore feeding concentrations at each operating stage during fluorite flotation, the ore feeding concentrations of fluorite sweep, fluorite selection and fluorite sweep are adjusted to 30% to 45%, and the ore feeding concentrations of fluorite sweep are adjusted to 30% to 45%, and the In the stage, an appropriate amount of acidified water glass and fatty acids are used as agents, and concentrated and dehydrated treatment is carried out to improve the effect of flotation agents and mineral particles.

Benefits of technology

It effectively improves the recovery rate of fluorite, reduces the dosage and cost of the drug, simplifies operations, and improves the universality and application value of the flotation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056573A_ABST
    Figure CN119056573A_ABST
Patent Text Reader

Abstract

The invention provides a flotation method for improving the fluorite recovery rate. The flotation method comprises the steps of fluorite roughing, fluorite scavenging, fluorite fine selection and fluorite fine scavenging. Wherein the fed ores of the fluorite scavenging, the fluorite fine selection and the fluorite fine scavenging are respectively subjected to concentration and dehydration treatment, and the concentration of the fed ores is increased to 30-45%. By means of the mode, effective intervention can be conducted on the ore feeding concentration in the fluorite scavenging operation stage, the fluorite concentration operation stage and the fluorite fine scavenging operation stage, all the operation stages are within the specific concentration range, it is guaranteed that flotation reagents can effectively collide with corresponding mineral particles within the concentration range, and the flotation efficiency is improved. And the acting effect between the flotation reagent and the minerals is improved, so that the fluorite recovery rate is effectively improved while the reagent dosage is reduced. Besides, the flotation method for improving the fluorite recovery rate is simple in overall operation and good in universality, compared with the prior art, more fluorite can be recovered with the lower agent cost, and the flotation method has the high practical application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorite flotation, and in particular to a flotation method for improving the recovery rate of fluorite. Background Art

[0002] At present, the domestic fluorite resources show the characteristics of many single deposits but small reserves, and a small number of associated deposits but large reserves. In associated deposits, fluorite is usually accompanied by minerals with similar properties such as calcite, barite, and celestite, which makes its separation and selection difficult and the cost of mineral selection high.

[0003] In order to efficiently recover fluorite resources, researchers have conducted extensive research on fluorite beneficiation technology and beneficiation reagents, and have developed a flotation process and reagent system that is more suitable for fluorite recovery. The current conventional fluorite flotation process flow chart is as follows: Figure 1 As shown in the figure, its main process adopts a short-process flotation process of one roughing and one sweeping, and multiple concentrations are carried out in the concentration stage, and high-grade fluorite concentrate products are obtained through concentrated return of middlings or concentrated re-selection of tailings.

[0004] In the existing fluorite flotation process, the flotation concentration at each stage is generally not subject to external interference and shows a natural decreasing change pattern. Normally, during fluorite flotation, the pulp concentration in the roughing operation stage is 28-40%, the pulp concentration in the cleaning operation stage is 20-30%, the pulp concentration in the scavenging operation stage is 15-20%, and the pulp concentration in the fine scavenging operation stage is 10-23%.

[0005] Among them, since the content of fluorite in the original ore is higher than that of ordinary metal minerals, the amount of flotation in the roughing is large, resulting in a rapid decrease in the scavenging concentration. When flotating fluorite in the scavenging operation stage, not only is the flotation efficiency low, but the recovery rate of fluorite scavenging is also much lower than that of other metal minerals, which affects the flotation recovery rate of fluorite. At the same time, in order to obtain high-quality fluorite concentrate, fluorite flotation needs to be refined 6 to 10 times, and the tailings need to be discharged in the first three times, resulting in a gradual decrease in the flotation concentration of fluorite during the selection process, especially in the first three times of selection operations, the phenomenon of fluorite falling off the trough is obvious, and the fluorite tailings of the fine scavenging operation have a tailing grade of 20 to 60%, or even higher, which seriously affects the recovery rate of fluorite.

[0006] However, for the above-mentioned problem of fluorite recovery rate being affected, the existing technology has not clarified the main reason for the affected recovery rate, nor has it systematically studied the effect of flotation concentration at each operation stage on fluorite recovery rate. The concentration at each operation stage in the current fluorite flotation process still maintains the law of natural decrease. Even if the grinding concentration is temporarily increased by concentration and dehydration to improve the grinding effect in the concentrate grinding stage, the removed water still needs to be merged back in the subsequent flotation process, and the actual flotation concentration has not changed. In order to improve the recovery rate of fluorite, the main research direction is still to improve the recovery rate of fluorite as much as possible by improving the process flow, improving the type of reagents, etc., but most of the existing improvement methods are costly and the effect of improving the recovery rate of fluorite is not significant enough.

[0007] In view of this, it is necessary to design an improved flotation method for improving the recovery rate of fluorite to solve the above problems. Summary of the invention

[0008] In view of the defects of the above-mentioned prior art, the object of the present invention is to provide a flotation method for improving the recovery rate of fluorite, by intervening in the feed concentration of each operation stage in the fluorite flotation process, and adjusting the feed concentration of each operation stage to a specific range to ensure that the flotation agent can efficiently react with the mineral particles, thereby effectively improving the recovery rate of fluorite while reducing the amount of agent used.

[0009] To achieve the above object, the present invention provides a flotation method for improving the recovery rate of fluorite, including fluorite roughing, fluorite scavenging, fluorite concentrating and fluorite fine scavenging;

[0010] The feed materials of the fluorite scavenging, fluorite concentrating and fluorite fine scavenging are respectively subjected to concentration and dehydration treatment to increase the feed concentration to 30% to 45%.

[0011] As a further improvement of the present invention, the flotation method for improving the recovery rate of fluorite provided by the present invention specifically comprises the following steps:

[0012] S1. Fluorite roughing: mixing the ore powder with water to obtain a primary slurry; performing a roughing operation on the primary slurry to obtain a fluorite rough concentrate and a fluorite roughing tailing;

[0013] S2. Fluorite scavenging: The fluorite rougher tailings are concentrated and dehydrated to obtain a scavenging feed with a concentration of 30% to 45%; the scavenging feed is scavenged to obtain a fluorite scavenging concentrate and fluorite tailings;

[0014] S3. Fluorite concentration: the fluorite coarse concentrate is concentrated and dehydrated to obtain a concentrated feed ore; the concentrated feed ore is subjected to a fine and rough separation operation to obtain a fluorite fine and rough separation concentrate and a fluorite concentrated tailings; and the fluorite fine and rough separation concentrate is further subjected to a concentration operation to obtain a fluorite concentrate;

[0015] S4. Fluorite fine scavenging: the fluorite selected tailings are concentrated and dehydrated to obtain fine scavenging feed ore; the fine scavenging feed ore is finely scavenged to obtain fluorite fine scavenging concentrate and fluorite tailings.

[0016] As a further improvement of the present invention, in step S3, the concentration of the concentrated feed ore is 30% to 40%.

[0017] As a further improvement of the present invention, in step S3, the reagents used in the fine and rough selection operations include: 350-1000 g / t of acidified water glass; the reagents used in each selection in the selection operation include: 0-800 g / t of acidified water glass.

[0018] As a further improvement of the present invention, in step S4, the concentration of the fine scavenging feed is 30% to 35%.

[0019] As a further improvement of the present invention, in step S4, the reagents used in the fine sweeping operation include: 200-300 g / t of acidified water glass and 10-30 g / t of fatty acid.

[0020] As a further improvement of the present invention, in step S2, the reagents used in the sweeping operation include: 200-500 g / t of acidified water glass and 20-100 g / t of fatty acid.

[0021] As a further improvement of the present invention, in step S1, the concentration of the primary slurry is 30% to 45%.

[0022] As a further improvement of the present invention, in step S1, the reagents used in the roughing operation include: 500-1200 g / t of soda ash, 1000-2000 g / t of acidified water glass, and 300-600 g / t of fatty acid.

[0023] As a further improvement of the present invention, the fluorite scavenging concentrate obtained in step S2 is returned to step S1 for the roughing operation.

[0024] The beneficial effects of the present invention are:

[0025] The flotation method for improving the recovery rate of fluorite provided by the present invention increases the feed concentration to a specific concentration range by concentrating and dehydrating the feed of fluorite scavenging, fluorite concentration and fluorite fine scavenging respectively, so that the flotation reagent can effectively collide with the corresponding mineral particles within the concentration range, thereby improving the effect of the flotation reagent and the mineral. Under this condition, the present invention can not only reduce the amount of reagents used in each operation stage, but also improve the operation recovery rate of each operation stage, thereby effectively improving the fluorite recovery rate while reducing the amount of reagents used. The flotation method for improving the recovery rate of fluorite provided by the present invention is simple to operate as a whole and has good universality. Compared with the prior art, it can recover more fluorite at a lower reagent cost and has a higher practical application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the conventional fluorite flotation process.

[0027] Figure 2 A schematic diagram of the process flow of the flotation method for improving fluorite recovery rate provided by the present invention.

[0028] Figure 3 It is a schematic diagram of the process flow of the fluorite sweeping operation stage in Examples 6 to 9 and Comparative Examples 1 to 3.

[0029] Figure 4 It is a schematic diagram of the process flow of the fluorite selection operation stage in Examples 10 to 12 and Comparative Examples 4 to 6.

[0030] Figure 5 It is a schematic diagram of the process flow of the fluorite fine sweeping operation stage in Examples 13 to 14 and Comparative Examples 7 to 9. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0033] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0034] In view of the problem of low fluorite recovery rate in the prior art, the present invention systematically studies the concentration of fluorite at each operation stage and finds that the concentration of fluorite at each operation stage has an important influence on the fluorite recovery rate. By adjusting the concentration of each key operation stage of the fluorite flotation process to a specific range, not only can the fluorite recovery rate be improved to ensure the maximum recovery of fluorite resources, but also the dosage of reagents can be reduced, effectively reducing the cost of reagents.

[0035] Based on the above research, the present invention provides a flotation method for improving the recovery rate of fluorite, including fluorite roughing, fluorite scavenging, fluorite concentrating and fluorite fine scavenging;

[0036] The feed materials of the fluorite scavenging, fluorite concentrating and fluorite fine scavenging are respectively subjected to concentration and dehydration treatment to increase the feed concentration to 30% to 45%.

[0037] It should be noted that the concentration and dehydration treatment refers to the use of thickening equipment to remove part of the water in the slurry to increase the feed concentration. The thickening equipment can be a cyclone, an inclined plate thickening box, a thickener, or other equipment can be selected according to actual conditions, as long as it can increase the feed concentration. The feed concentration mentioned in the present invention represents the mass concentration of the mineral powder particles in the slurry, which will not be repeated below.

[0038] Through the above-mentioned method, the present invention can effectively overcome the law of natural concentration reduction in each operation stage in the conventional fluorite flotation process, and accurately control the feed concentration of fluorite scavenging, fluorite concentration and fluorite fine scavenging operation stages in the flotation process to a specific range, so that the flotation agent can efficiently react with the mineral particles, thereby effectively improving the recovery rate of fluorite while reducing the dosage of the agent.

[0039] More specifically, Figure 2 As shown, in some embodiments of the present invention, the flotation method for improving the recovery rate of fluorite specifically includes the following steps:

[0040] S1. Fluorite roughing

[0041] The fluorite ore to be selected is ground to obtain ore powder; the ore powder is mixed with water to obtain a primary slurry. The mass fraction of the ore powder in the primary slurry is preferably 30% to 45%, and the solid particles with a particle size of less than 0.074 mm in the primary slurry account for more than 70% of the total mass of the ore powder.

[0042] Then, the primary slurry is subjected to a roughing operation, which specifically includes the following steps:

[0043] Soda ash is added to the primary pulp and stirred for 3 minutes, then acidified water glass is added to the pulp and stirred for 2 minutes, and then fatty acid is added to the pulp and stirred for 3 minutes. The reagent is fully reacted with the mineral surface through the stirring process, and then roughing is carried out for 5 minutes to obtain fluorite rough concentrate and fluorite roughing tailings.

[0044] The acidified water glass in the present invention is prepared by mixing 5% dilute sulfuric acid and 20% water glass in a mass ratio of 1:1 to 3:1, which will not be described in detail below.

[0045] Generally, when the mass fraction of the mineral powder in the primary slurry is less than 30%, the amount of each reagent used in the roughing operation is: 1000-3000 g / t of soda ash, 1500-3000 g / t of acidified water glass, and 800-1000 g / t of fatty acid. The present invention increases the mass fraction of the mineral powder in the primary slurry to 30%-45%, and the amount of each reagent used in the roughing operation is preferably: 500-1200 g / t of soda ash, 1000-2000 g / t of acidified water glass, and 300-600 g / t of fatty acid. Compared with the use of a low-concentration primary slurry, the amount of reagent used is significantly reduced, and the recovery rate of fluorite in the roughing operation stage can be improved.

[0046] S2. Fluorite Sweeping

[0047] The fluorite roughing tailings obtained in step S1 are concentrated and dehydrated to obtain scavenging feed with a concentration of 30% to 45%.

[0048] Then, the scavenging feed is subjected to a scavenging operation, which specifically includes the following steps:

[0049] Acidified water glass is added to the concentrated and dehydrated scavenging feed, stirred for 2 minutes, and then fatty acid is added to the slurry and stirred for 2 minutes. The reagent is fully reacted with the mineral surface through the stirring process, and then scavenging is performed for 3 minutes to obtain fluorite scavenging concentrate and fluorite tailings. The fluorite scavenging concentrate is returned to the roughing operation in step S1.

[0050] Normally, when the concentration of the scavenging feed is 15% to 20%, the amount of each reagent used during the scavenging operation is: 500 to 1500 g / t of acidified water glass, 100 to 300 g / t of fatty acid. In the present invention, after the concentration of the scavenging feed is increased to 30% to 45%, the amount of each reagent used during the scavenging operation is preferably: 200 to 500 g / t of acidified water glass, 20 to 100 g / t of fatty acid, which significantly reduces the amount of reagents used compared to when no concentration and dehydration is performed, and can improve the recovery rate of fluorite in the scavenging operation stage.

[0051] S3. Fluorite Selection

[0052] The fluorite rough concentrate obtained in step S1 is used as the selected feed ore. If the concentration of the fluorite rough concentrate is lower than 30%, the fluorite rough concentrate needs to be concentrated and dehydrated, and the concentration of the selected feed ore is preferably increased to 30% to 40%.

[0053] In the present invention, it is preferred to use multiple concentration methods to concentrate fluorite, and more preferably one fine and rough concentration operation and six concentration operations, and the specific method is:

[0054] The selected ore is subjected to a fine-roughing operation to obtain a fluorite fine-roughing concentrate and a fluorite selected tailings; and the fluorite fine-roughing concentrate is subjected to six concentration operations to obtain a fluorite concentrate.

[0055] Among them, the reagents used in the rough and fine selection operations are acidified water glass. After adding the acidified water glass, stir for 2 minutes, and then carry out rough and fine selection or fine selection for 4 minutes.

[0056] Normally, when the concentration of the selected feed is lower than 30%, the amount of acidified water glass used in the fine and rough selection operation is 500-2000 g / t, and the amount of acidified water glass used in each selection operation is 0-1000 g / t, and the amount of acidified water glass used is gradually decreasing. The present invention increases the concentration of the selected feed to 30%-40%, and the amount of acidified water glass used in the fine and rough selection operation is preferably 350-1000 g / t, and the amount of acidified water glass used in the selection operation is preferably 0-800 g / t, and the amount of acidified water glass used is gradually decreasing. Compared with the case where no concentration and dehydration is performed, the amount of reagent used is significantly reduced, and the recovery rate of fluorite in the fluorite selection stage can be improved.

[0057] S4. Fluorite Precision Sweeping

[0058] The fluorite concentrate tailings obtained in step S3 are concentrated and dehydrated to obtain a fine scavenging feed with a concentration of 30% to 35%.

[0059] Then, the fine sweeping operation is performed on the fine sweeping feed, and the fine sweeping operation specifically includes the following steps:

[0060] Acidified water glass is added to the concentrated and dehydrated fine scavenging feed, stirred for 2 minutes, and then fatty acid is added to the pulp and stirred for 2 minutes. The reagent is fully reacted with the mineral surface through the stirring process, and then fine scavenging is carried out for 4 minutes to obtain fluorite fine scavenging concentrate and fluorite tailings. The fluorite fine scavenging concentrate is returned to the fine roughing operation or the concentrating operation.

[0061] Generally, when the concentration of the fine scavenging feed is 10% to 23%, the amount of each reagent used in the fine scavenging operation is preferably: 300 to 500 g / t of acidified water glass, 50 to 150 g / t of fatty acid. The present invention increases the concentration of the fine scavenging feed to 30% to 35%, and the amount of each reagent used in the fine scavenging operation is preferably: 200 to 300 g / t of acidified water glass, 10 to 30 g / t of fatty acid, which significantly reduces the amount of reagents used compared to when no concentration and dehydration is performed, and can improve the recovery rate of fluorite in the fine scavenging operation stage.

[0062] Through the above-mentioned method, the present invention can effectively intervene in the feed concentration of fluorite scavenging, fluorite concentration and fluorite fine scavenging operations by means of concentration and dehydration, and increase the feed concentration of each operation stage to a specific range, so as to ensure that the flotation agent can effectively collide with the surface of the fluorite mineral within the concentration range, improve the effect of the flotation agent on the fluorite, and then improve the recovery rate of the fluorite, while reducing the amount of the flotation agent.

[0063] The flotation method for improving the recovery rate of fluorite provided by the present invention is described in detail below with reference to specific embodiments and comparative examples.

[0064] Example 1

[0065] This embodiment provides a flotation method for improving fluorite recovery rate, comprising the following steps:

[0066] S1. Fluorite roughing

[0067] The fluorite ore to be selected is ground to obtain ore powder; the ore powder is mixed with water to obtain a primary slurry with a ore powder concentration of 35%, in which solid particles with a particle size of less than 0.074 mm account for more than 70% of the total mass of the ore powder.

[0068] Then, the primary slurry is subjected to a roughing operation, which specifically includes the following steps:

[0069] Add 1200g / t of soda ash to the primary pulp and stir for 3 minutes, then add 1500g / t of acidified water glass to the pulp and stir for 2 minutes, then add 500g / t of fatty acid to the pulp and stir for 3 minutes. The stirring process allows the reagent to fully react with the mineral surface, and then perform roughing for 5 minutes to obtain fluorite rough concentrate and fluorite roughing tailings. The acidified water glass is made by mixing 5% dilute sulfuric acid and 20% water glass in a mass ratio of 2:1.

[0070] S2. Fluorite Sweeping

[0071] The fluorite roughing tailings obtained in step S1 are connected to a thickener through a pipeline for concentration and dehydration. The overflow water of the thickener can be returned to the roughing operation as water mixed with the mineral powder, and the underflow is used as scavenging feed to enter the scavenging operation. The concentration of the scavenging feed is controlled to be 35%.

[0072] Then, the scavenging feed is subjected to a scavenging operation, which specifically includes the following steps:

[0073] 400 g / t of acidified water glass was added to the scavenging feed, stirred for 2 minutes, and then 25 g / t of fatty acid was added to the pulp, stirred for 2 minutes. The reagent was fully reacted with the mineral surface through the stirring process, and then scavenging was performed for 3 minutes to obtain fluorite scavenging concentrate and fluorite tailings. The fluorite scavenging concentrate was returned to the roughing operation in step S1.

[0074] S3. Fluorite Selection

[0075] The fluorite rough concentrate obtained in step S1 is concentrated and dehydrated: the fluorite rough concentrate is connected to the first-stage cyclone together with the foam washing water. After the fluorite rough concentrate is concentrated by the first-stage cyclone, the sand is settled and enters the subsequent operation, and the overflow is connected to the second-stage cyclone. After the second-stage cyclone is concentrated, the overflow is directly discharged into the tailings. The sand settling of the second-stage cyclone is combined with the sand settling of the first-stage cyclone as the selected feed ore, which enters the fluorite selection operation. By adjusting the pressure of the first-stage cyclone and the second-stage cyclone and the size of the sand settling port, the concentration of the selected feed ore is controlled to 35%.

[0076] Then, a fine-roughing operation is performed on the selected ore, the amount of acidified water glass used in the fine-roughing operation is 800g / t, the acidified water glass is added and stirred for 2 minutes, and then a fine-roughing operation is performed for 4 minutes to obtain fluorite fine-roughing concentrate and fluorite selected tailings; the fluorite fine-roughing concentrate is subjected to six selections to obtain fluorite concentrate, and the amounts of acidified water glass used in the selection one, selection two, selection three, selection four, selection five and selection six operations are 800g / t, 600g / t, 400g / t, 200g / t, 100g / t and 0g / t respectively, each time the acidified water glass is added, stirring is performed for 2 minutes, and then selection is performed for 4 minutes, and the middlings produced in each selection are returned to the previous operation to finally obtain fluorite concentrate.

[0077] S4. Fluorite Precision Sweeping

[0078] The fluorite concentrate tailings obtained in step S3 are concentrated and dehydrated: the fluorite concentrate tailings are connected to the inclined plate thickener through a pipeline, the overflow water of the inclined plate thickener is returned to the flotation operation as replenishing water, and the bottom flow is used as fine scavenging feed to enter the fine scavenging operation, and the concentration of the fine scavenging feed is controlled to be 35%.

[0079] Then, the fine sweeping operation is performed on the fine sweeping feed, and the fine sweeping operation specifically includes the following steps:

[0080] Add 250g / t of acidified water glass to the fine scavenging feed and stir for 2 minutes, then add 20g / t of fatty acid to the pulp and stir for 2 minutes. The stirring process allows the reagent to fully react with the mineral surface, and then carry out fine scavenging for 4 minutes to obtain fluorite fine scavenging concentrate and fluorite tailings. The fluorite fine scavenging concentrate is returned to the fine and roughing operation.

[0081] After flotation is performed according to the above method, the final flotation results are shown in Table 1.

[0082] Table 1 Flotation results of Example 1 (%)

[0083]

[0084]

[0085] It can be seen from Table 1 that based on the flotation method provided by the present invention, a higher recovery rate of fluorite (CaF2) can be achieved.

[0086] In order to further analyze the effect of feed concentration in each operation stage on fluorite recovery rate and reagent dosage, separate experiments were conducted on fluorite roughing, fluorite scavenging, fluorite concentrating and fluorite fine scavenging operations.

[0087] Embodiments 2 to 5

[0088] Examples 2 to 5 respectively provide a method for roughing fluorite, and the raw ore used is quartz vein type fluorite ore. The method used is consistent with the fluorite roughing method in Example 1, except that different dosages of reagents are used according to different primary slurry concentrations. The flotation conditions and flotation results of Examples 2 to 5 are shown in Table 2.

[0089] Table 2 Flotation conditions and flotation results of Examples 2 to 5 (%)

[0090]

[0091] It can be seen from Table 2 that with the increase of flotation concentration, the overall dosage of reagents in the fluorite flotation process shows a downward trend, the dosage of soda ash has decreased by 1 / 3, the dosage of acidified water glass has decreased by 10%, and the dosage of fatty acids has decreased by 1 / 3. The flotation recovery rate of fluorite increases with the increase of concentration. When the concentration is increased to 45%, the fluorite recovery rate is increased by 26.26 percentage points compared with the concentration of 30%. The implementation effect is very significant.

[0092] Examples 6 to 9 and Comparative Examples 1 to 3

[0093] Examples 6 to 9 and Comparative Examples 1 to 3 respectively provide a method for scavenging fluorite, using fluorite roughing tailings as feed ore, and the process flow diagram thereof is shown in FIG. Figure 3 As shown, it is consistent with the fluorite scavenging method in Example 1, except that the feed concentration and the dosage of the reagent are adjusted. The flotation conditions and flotation results of Examples 6 to 9 and Comparative Examples 1 to 3 are shown in Table 3.

[0094] Table 3 Flotation conditions and flotation results of Examples 6 to 9 and Comparative Examples 1 to 3 (%)

[0095]

[0096] It can be seen from Table 3 that: as the flotation concentration increases, compared with the flotation concentration of Comparative Example 1, the dosage of acidified water glass and fatty acid shows an overall downward trend, while the recovery rate of fluorite shows an upward trend; after the concentration reaches 45%, the fluorite recovery rate increases by 26.26 percentage points compared with Comparative Example 1, the dosage of fatty acid decreases by 50%, and the dosage of acidified water glass decreases by 50%; after the concentration reaches 50%, the grade of fluorite concentrate in Comparative Example 3 is lower than 30%, and the dosage of acidified water glass further increases, which shows that the flotation concentration should not exceed 50%.

[0097] Examples 10 to 12 and Comparative Examples 4 to 6

[0098] Examples 10 to 12 and Comparative Examples 4 to 6 respectively provide a method for concentrating fluorite, using fluorite coarse concentrate as feed ore, and the process flow diagram thereof is shown in FIG. Figure 4 As shown, it is consistent with the primary fluorite fine and rough selection method in Example 1, except that the feed concentration and the dosage of the reagent are adjusted. The flotation conditions and flotation results of Examples 10 to 12 and Comparative Examples 4 to 6 are shown in Table 4.

[0099] Table 4 Flotation conditions and flotation results of Examples 10 to 12 and Comparative Examples 4 to 6 (%)

[0100]

[0101] It can be seen from Table 4 that: with the increase of flotation concentration, compared with the flotation concentration of Comparative Examples 4 and 5, the dosage of acidified water glass and fatty acid shows an overall downward trend, while the recovery rate of fluorite shows an upward trend; after the concentration reaches 40%, the fluorite recovery rate is 17.52 percentage points higher than that of Comparative Example 4, and the dosage of acidified water glass is reduced by 41.67%; the recovery rate is 7.81 percentage points higher than that of Comparative Example 5, and the dosage of acidified water glass is reduced by 36.36%; after the concentration reaches 45%, the fluorite concentrate grade and recovery rate in Comparative Example 5 have no advantages, and the dosage of acidified water glass increases.

[0102] Examples 13 to 14 and Comparative Examples 7 to 9

[0103] Examples 13 to 14 and Comparative Examples 7 to 9 respectively provide a method for fine scavenging of fluorite, using fluorite roughing tailings as feed ore, and the process flow diagram thereof is shown in FIG. Figure 5 As shown, it is consistent with the fluorite fine scavenging method in Example 1, except that the feed concentration and the dosage of the reagent are adjusted. The flotation conditions and flotation results of Examples 13 to 14 and Comparative Examples 7 to 9 are shown in Table 5.

[0104] Table 5 Flotation conditions and flotation results of Examples 13 to 14 and Comparative Examples 7 to 9 (%)

[0105]

[0106] It can be seen from Table 5 that: with the increase of flotation concentration, compared with the flotation concentration of Comparative Examples 7 and 8, the dosage of acidified water glass and fatty acid shows an overall downward trend, while the recovery rate of fluorite shows an upward trend; after the concentration reaches 35%, the fluorite recovery rate is 41.49 percentage points higher than that of Comparative Example 7, the dosage of acidified water glass is reduced by 40%, and the dosage of fatty acid is reduced by 70%, and the recovery rate is 34.85 percentage points higher than that of Comparative Example 8, the dosage of acidified water glass is reduced by 40%, and the dosage of fatty acid is reduced by 62.5%; after the concentration exceeds 40%, the fluorite concentrate grade and recovery rate in Comparative Example 9 have no advantages, and the dosage of acidified water glass increases.

[0107] In summary, the present invention provides a flotation method for improving the recovery rate of fluorite, including fluorite roughing, fluorite scavenging, fluorite concentrating and fluorite fine scavenging; wherein, the feed of the fluorite scavenging, fluorite concentrating and fluorite fine scavenging is respectively concentrated and dehydrated to increase the feed concentration to 30% to 45%. Through the above-mentioned method, the present invention can effectively intervene in the feed concentration of the fluorite scavenging, fluorite concentrating and fluorite fine scavenging operation stages, so that each operation stage is within a specific concentration range, so as to ensure that the flotation reagent can effectively collide with the corresponding mineral particles within the concentration range, improve the effect of the flotation reagent and the mineral, thereby effectively improving the fluorite recovery rate while reducing the dosage of the reagent. In addition, the flotation method for improving the recovery rate of fluorite provided by the present invention is simple to operate as a whole and has good universality. Compared with the prior art, it can recover more fluorite at a lower reagent cost and has a higher practical application value.

[0108] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A flotation method for improving fluorite recovery, characterized in that: Including fluorite rough selection, fluorite sweeping selection, fluorite concentrating and fluorite fine sweeping selection; The feed materials of the fluorite scavenging, fluorite concentrating and fluorite fine scavenging are respectively subjected to concentration and dehydration treatment to increase the feed concentration to 30% to 45%.

2. The flotation method for improving fluorite recovery rate according to claim 1, characterized in that: The specific steps include: S1. Fluorite roughing: mixing the ore powder with water to obtain a primary slurry; performing a roughing operation on the primary slurry to obtain a fluorite rough concentrate and a fluorite roughing tailing; S2. Fluorite scavenging: The fluorite rougher tailings are concentrated and dehydrated to obtain a scavenging feed with a concentration of 30% to 45%; the scavenging feed is scavenged to obtain a fluorite scavenging concentrate and fluorite tailings; S3. Fluorite concentration: the fluorite coarse concentrate is concentrated and dehydrated to obtain a concentrated feed ore; the concentrated feed ore is subjected to a fine and rough separation operation to obtain a fluorite fine and rough separation concentrate and a fluorite concentrated tailings; and the fluorite fine and rough separation concentrate is further subjected to a concentration operation to obtain a fluorite concentrate; S4. Fluorite fine scavenging: the fluorite selected tailings are concentrated and dehydrated to obtain fine scavenging feed ore; the fine scavenging feed ore is finely scavenged to obtain fluorite fine scavenging concentrate and fluorite tailings.

3. The flotation method for improving fluorite recovery rate according to claim 2, characterized in that: In step S3, the concentration of the concentrated feed ore is 30% to 40%.

4. The flotation method for improving fluorite recovery rate according to claim 3, characterized in that: In step S3, the reagents used in the rough and fine separation operations include: 350-1000 g / t of acidified water glass; the reagents used in each selection in the fine separation operation include: 0-800 g / t of acidified water glass.

5. The flotation method for improving fluorite recovery rate according to claim 2, characterized in that: In step S4, the concentration of the fine scavenging feed is 30% to 35%.

6. The flotation method for improving fluorite recovery rate according to claim 5, characterized in that: In step S4, the reagents used in the fine sweeping operation include: 200-300 g / t of acidified water glass and 10-30 g / t of fatty acid.

7. The flotation method for improving fluorite recovery rate according to claim 2, characterized in that: In step S2, the reagents used in the sweeping operation include: 200-500 g / t of acidified water glass and 20-100 g / t of fatty acid.

8. The flotation method for improving fluorite recovery rate according to claim 2, characterized in that: In step S1, the concentration of the primary slurry is 30% to 45%.

9. The flotation method for improving fluorite recovery rate according to claim 8, characterized in that: In step S1, the reagents used in the roughing operation include: 500-1200 g / t of soda ash, 1000-2000 g / t of acidified water glass, and 300-600 g / t of fatty acid.

10. The flotation method for improving fluorite recovery rate according to claim 2, characterized in that: The fluorite scavenging concentrate obtained in step S2 is returned to the roughing operation in step S1.

Citation Information

Patent Citations

  • Fluorite ore separation method adopting scavenging concentration and desliming

    CN106076605A

  • Floatation method for restraining silicate gangue minerals in fluorine mine

    CN107638959A

  • Mineral processing technology for recycling tungsten and fluorite from low-grade tungsten flotation high-calcium rough concentrate

    CN108435429A

  • Inhibitor for high-calcium fluorite flotation as well as preparation method and application process of inhibitor

    CN113560031A

  • Beneficiation of fluorspar ore

    US4043455A

Cited By

  • Method for flotation of fluorite in dolomite type fluorite mine

    CN120838565A