Battery cell screening method
The lithium battery cells are screened through pulse discharge method, and abnormal battery cells are screened using voltage change curves, which solves the problem of low screening efficiency in the existing technology, and accurately screen abnormal battery cells in a short time, improving battery cell quality control , reduces production costs.
Patent Information
- Application Number
- CN202411324748.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to effectively screen out lithium battery cells with abnormal self-discharge in a short period of time, resulting in these abnormal battery cells flowing into the next process or in the hands of customers with the normal battery cells, affecting the service life and function of the battery pack.
The pulse discharge method is used to divide the battery cell into capacity and charge it at the first rate, then pulse discharge at the second rate (20C~30C), and the battery cell is adjusted to a specific SOC level, and then left to stand for 0.5 hours to 2 hours. Draw the voltage over time curve to screen out abnormal cells.
Through pulse discharge, accelerate the chemical dissolution short circuit process of the battery cell, generate polarization and layer the voltage, significantly improve the screening efficiency of abnormal battery cells, shorten the screening time, reduce costs, avoid resource waste and abnormal battery cells flow into customers' hands risk.
Smart Images

Figure CN119056765A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a battery cell screening method. Background Art
[0002] With the rapid development of the electric vehicle industry, advantages such as high energy density, high power, high safety, and long life have gradually become the core energy components of electric vehicles. Due to the limitations of battery capacity and power, the power battery system of electric vehicles is often composed of dozens or hundreds of lithium-ion batteries connected in series and parallel. However, due to factors such as production processes and material differences, each battery is prone to differences in internal resistance, life, voltage, self-discharge rate and other performance. When these battery packs composed of cells with different performance are used, the performance differences of the battery cells will be further amplified due to the different use environments of the battery cells in the battery pack, which will accelerate the attenuation of the battery pack performance, and as the use process continues, the service life of the battery pack will be further reduced.
[0003] Before using the battery, it is usually necessary to test and screen the cells to be used to select cells with stable performance. In the process of screening abnormal cells, it is particularly important to select batteries with abnormal self-discharge. However, in the prior art, screening batteries with abnormal self-discharge usually requires the cells to be left standing for 7 days. The method of screening cells according to the change of K value has a long screening time and low efficiency. Moreover, this method can only screen out the vast majority of abnormal self-discharge cells caused by physical short circuits. Those cells with abnormal self-discharge caused by chemical short circuits cannot be screened out by standing for 7 days to test the K value. Instead, the battery needs to be left standing for a very long time after 3 to 6 months to show the phenomenon of voltage reduction. However, due to the efficiency requirements, the cells may not be left standing for such a long time, so these cells with abnormal self-discharge will flow into the next process or the hands of customers together with normal cells, thereby affecting the actual service life and function of the battery pack due to the use of these abnormal cells. Therefore, how to design a method to screen out cells with abnormal self-discharge in a short time is an urgent problem to be solved for the control of cell quality. Summary of the invention
[0004] In order to solve the technical problem in the prior art that it is difficult to screen out batteries with abnormal self-discharge in a short time, the present invention provides a battery screening method comprising the following steps: S1: Take out multiple batteries to be used; S2: dividing the capacity of each battery cell taken out in step S1; S3: pulse discharge each battery cell; S4: After the battery cells undergoing the pulse test in step S3 are left to stand, a curve of the voltage of each battery cell changing with time is plotted; S5: Filter out abnormal cells according to the voltage stratification of each cell in the voltage variation curve over time drawn in step S4.
[0005] Furthermore, the pulse discharge in step S3 includes the following steps: first, charging each battery cell at a first rate; then, pulse discharging each battery cell at a second rate; and finally, continuing to discharge each battery cell at a third rate to adjust the battery cell to the SOC level after the capacity division in step S2.
[0006] Furthermore, the second magnification is greater than the first magnification.
[0007] Furthermore, in the step S3, the second ratio is 20°C to 30°C.
[0008] Furthermore, in step S3, the battery cell is discharged at the second rate pulse for a time period of 0.1 seconds to 10 seconds.
[0009] Furthermore, in the step S2, the capacity of the battery cell is divided to 30% to 40% of the initial SOC of the battery cell.
[0010] Furthermore, the battery cell in step S4 is left standing for 0.5 hours to 2 hours.
[0011] The battery cell screening method of the present invention accelerates the process of chemical dissolution and short-circuiting of hidden danger battery cells through pulsed large current discharge. At the same time, the polarization generated by the pulse discharge will make the battery cell voltage lower than the original potential. In the process of static depolarization, since the ion transmission speed inside the chemical short-circuited battery cell is faster, the voltage recovery phenomenon caused by depolarization is more obvious. The voltage values of normal battery cells and hidden danger battery cells can be stratified in a short time to screen out abnormal battery cells, avoid wasting resources caused by long-term static storage, and reduce the risk of abnormal battery cells flowing into the hands of customers. Abnormal battery cells can be screened out in advance, which improves the efficiency of abnormal battery cell screening and reduces the cost of battery cell screening. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a curve diagram showing the change of the cell voltage over time after the cell is subjected to a pulse test in the cell screening method of the present invention; Figure 2 A distribution diagram of cell voltage and K value for verifying the reliability of the cell screening method of the present invention; Figure 3 A curve diagram of the change of K value and time drawn for a normal battery cell in order to verify the reliability of the battery cell screening method of the present invention; Figure 4 A curve diagram of the change of K value and time drawn for the battery cells of group B in order to verify the reliability of the battery cell screening method of the present invention; Figure 5A curve diagram of the change in K value versus time drawn for the C group cells in order to verify the reliability of the cell screening method of the present invention. DETAILED DESCRIPTION
[0013] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0014] The cell screening method of this embodiment mainly includes the following steps: S1: Take out multiple battery cells to be used from the warehouse (take battery cells with K value greater than zero and less than 0.07).
[0015] S2: Divide the capacity of each battery cell in step S1 to 35% of the initial SOC.
[0016] S3: Performing a pulse test on each battery cell in step S2, the pulse test comprising the following steps: D1: Charge each cell at 1C rate to 15% SOC until each cell reaches 50% SOC; D2: Each cell is then pulse-discharged at a rate of 30C for 5 seconds; D3: Continue to discharge each battery cell at 1C rate in step D3 to adjust the capacitance of each battery cell to the initial SOC of 35%.
[0017] S4: Each battery after step S3 is left to stand for a period of time and the curves of each battery cell changing with voltage and time during the standing period are monitored. In this embodiment, the battery cell is left to stand for 2 hours and the following curves are plotted: Figure 1 The cell voltage is shown as a function of time.
[0018] S5: According to the curve of cell voltage variation over time drawn in step S4, the abnormal cells are selected.
[0019] In this embodiment, after the pulse test, the battery cell is left to stand for a period of time, and the battery cell voltage will recover quickly and stabilize after a period of time. In this embodiment, it is specifically manifested as follows: within 600 seconds after the pulse discharge, the voltage is in a rapid recovery period, and then during the period of 600-1000s, the rate of voltage recovery slows down and stabilizes at the 1000th second. However, as the standing time of each battery cell increases, especially after standing for about 30 minutes, the battery cell voltage shows obvious stratification; the voltage of the normal battery cell is lower than the specific value of 3.285V; the voltage of another group of battery cells (abnormal battery cells) is significantly higher than the specific value of 3.285V.
[0020] Combining the curve of the voltage change over time after pulse charge and discharge of the battery cell with the existing theoretical research, it is found that: Abnormal cells usually have micro short circuits caused by metal foreign matter mixed into the positive electrode, which is oxidized and dissolved under high voltage; however, they may also be reduced and accumulated at low potential of the negative electrode through diffusion of the electrolyte, eventually causing the diaphragm to conduct and form micro short circuits. The self-discharge abnormality caused by this short circuit is difficult to screen out through conventional K value tests in a short period of time, and the difference is generally reflected after a long period of static standing. The cell screening method of this embodiment accelerates the process of chemical dissolution and short circuit of metal particles inside the battery by discharging the battery with a large pulse current; after high current discharge, the voltage of this cell will deviate from the original potential due to polarization; at the same time, during the static depolarization process, due to the faster ion transmission speed inside the cell with chemical short circuit, the depolarization causes the voltage to recover faster, the phenomenon is more obvious, and the voltage is at a higher potential; in contrast, those cells without short circuits inside the battery are relatively slow in depolarization due to the obstruction of charge transmission, and the voltage is at a lower potential. Therefore, in this embodiment, after the battery cells are pulse discharged, the voltage values of abnormal battery cells and normal battery cells can be clearly stratified in a short period of time. The battery cells with high voltage are potential battery cells with performance defects such as internal micro-short circuits, while the battery cells with low voltage are normal battery cells without internal micro-short circuits.
[0021] At the same time, in the battery cell screening process of the present invention, we continuously change the various parameter settings in the battery cell screening process, and find that in step S3, each battery cell is discharged at a rate of 20C~30C for 0.1 second-10 seconds, and after standing, the voltage of normal battery cells and abnormal battery cells can be obviously stratified, and the normal battery cells and abnormal battery cells can be selected. In step S2, each battery cell is divided into a capacity within the range of 30%-40% of the original SOC of the battery cell, and then the battery cell is pulse-discharged in step S3, which can obviously achieve the voltage stratification of normal battery cells and abnormal battery cells, and the abnormal battery cells can be sorted out. After the battery cell is pulse-discharged, it is left to stand for 0.5h-2h, and the voltage stratification phenomenon can be obviously achieved.
[0022] In order to verify whether the method of screening cells according to the change of cell voltage over time after pulse testing of the cells is reliable, we further verified it by using the existing commonly used cell screening methods. The verification methods include the following two methods: Verification method 1 (voltage change of battery cells after long-term storage): All the battery cells to be selected are stored in the warehouse for half a year and then the voltage of each battery cell is tested. Figure 2 The correlation distribution diagram of the cell voltage and K value is shown. Figure 2It can be seen that in the overall cell voltage distribution, 3100 mV serves as the dividing line. Among them, the cells with a voltage of 3100 mV show a scattered distribution, while those with a voltage above 3100 mV exhibit a concentrated distribution. By comparing the results of the cell voltage change over time after the pulse test described in this embodiment, it is found that: for the abnormal cells with a voltage higher than the specific value of 3.29 V after standing for two hours after the pulse test, all of them show a significant voltage drop after standing for half a year, and are all lower than 3100 mV. We further divided these abnormal cells into Group B and Group C according to the K value and voltage of the cells. Among them, Group B has K < 0.045; Group C has 0.045 < K < 0.065; normal cells are divided into Group A (i.e., voltage value greater than 3100 mV).
[0023] Verification method 2 (seven-day K value test): Re-measure the K value of each group of cells after grouping by verification method 1. The specific K value measurement method is as follows: After standing each cell for 24 h, measure the OCV1 of each cell, and then measure the voltage of the cell every 24 h for 7 consecutive days, a total of 8 times and record them as OCV1~OCV8 respectively; at the same time, calculate the K value at different standing days through the formula Kx = (COV1 - OCVx + 1) / 24x (where x is the standing day), and obtain the change curve of the K value of each group of cells over time. As Figure 3-5 shown: The change in the K value of Group A cells (normal cells) after standing for 1 to 7 days is not significant, but the K2 value of the abnormal cells in Group B and Group C will suddenly increase on the third day of standing.
[0024] By comparing the cell screening method of the present invention with the existing cell screening methods 1 and 2, the cell screening method of the present invention can greatly reduce the time for screening abnormal cells. The existing screening method takes 3 - 6 months to completely screen out abnormal cells, while the screening method of the present invention can screen out the cells with micro-short circuits inside within 2 hours, greatly shortening the screening time, and the screening accuracy is equivalent to the efficiency of the existing 3 - 6 months of standing time. Therefore, it greatly improves the efficiency of the existing abnormal cell screening, reduces production costs, and controls the consistency of product quality.
[0025] The cell screening method of the present invention accelerates the process of chemical dissolution short circuit of potential hazard cells through pulsed high-current discharge. At the same time, the polarization generated by pulsed discharge will make the cell voltage lower than the original potential. During the process of standing for depolarization, due to the faster ion transport speed inside the chemically short-circuited cells, the voltage recovery phenomenon caused by depolarization is more obvious, and the voltage values of normal cells and potential hazard cells can be stratified within a short time; it avoids the waste of resources caused by long-term standing, and at the same time reduces the risk of abnormal cells flowing into the hands of customers, can screen out abnormal cells in advance, improves the efficiency of abnormal cell screening, and reduces the cost of cell screening.
[0026] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for screening battery cells, characterized in that: The following steps are involved: S1: Take out multiple batteries to be used; S2: dividing the capacity of each battery cell taken out in step S1; S3: pulse discharge each battery cell; S4: After the battery cells undergoing the pulse test in step S3 are left to stand, a curve of the voltage of each battery cell changing with time is plotted; S5: Filter out abnormal cells according to the voltage stratification of each cell in the voltage variation curve over time drawn in step S4.
2. The battery cell screening method according to claim 1, characterized in that: The pulse discharge in step S3 includes the following steps: first, charging each battery cell at a first rate; then, pulse discharging each battery cell at a second rate; and finally, continuing to discharge each battery cell at a third rate to adjust the battery cell to the SOC level after the capacity division in step S2.
3. The cell screening method as claimed in claim 2, characterized in that: The second magnification is greater than the first magnification.
4. The battery cell screening method according to claim 3, characterized in that: In the step S3, the second magnification is 20°C to 30°C.
5. The battery cell screening method according to claim 2, characterized in that: In the step S3, the battery cell is discharged at the second rate pulse for a time period of 0.1 seconds to 10 seconds.
6. The battery cell screening method according to claim 1, characterized in that: In the step S2, the battery cell is divided into 30% to 40% of the initial SOC of the battery cell.
7. The battery cell screening method according to claim 1, characterized in that: The battery cell in step S4 is left to stand for 0.5 hours to 2 hours.