2024-10-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The temperature stability of high-steel pipeline steel is difficult to control when coiled at lower temperatures, affecting its toughness and performance.

Method used

By optimizing the finish rolling and laminar flow cooling process, the coiling temperature of the middle part of the steel coil is controlled at 380±20℃, the front-section centralized cooling and curing laminar flow cooling boiling water mode is adopted, and the rolling speed and cooling water volume are controlled in stages to ensure laminar flow The cooling water temperature is between 28°C and 32°C, and the surface water of the steel plate is completely purged by side water spraying.

Benefits of technology

The stable control of the coiling temperature of high-steel pipeline steel is achieved, and the performance uniformity of pipeline steel and the safety performance of natural gas pipelines are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056889A_ABST
    Figure CN119056889A_ABST
Patent Text Reader

Abstract

The invention discloses a stable control method for low coiling temperature of acicular ferrite type thick pipeline steel, and belongs to the technical field of metallurgy. The stable control method comprises the steps that the coiling temperature of the middle part of a steel coil is stably controlled to be 380 + / -20 DEG C by optimizing a finish rolling and laminar cooling process, coiling is conducted, and the needle-shaped ferrite type thick-specification pipeline steel is prepared, specifically, the initial rolling temperature is controlled to be 910 + / -10 DEG C in the finish rolling procedure, and the final rolling temperature is controlled to be 795 + / -15 DEG C in the finish rolling procedure; the laminar cooling process adopts a front-section centralized cooling and boiling water curing mode, and the laminar cooling process is divided into a forced cooling section and a conventional cooling section for cooling by controlling the number of cooling nozzles of an upper header and a lower header. By the adoption of the stability control method, the problem that the temperature stability of the high-grade pipeline steel is difficult to control when the high-grade pipeline steel is coiled at the low temperature can be effectively solved, and the performance uniformity of the pipeline steel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, relates to a production method of hot-rolled high-grade pipeline steel, and specifically relates to a stable control method for low coiling temperature of acicular ferrite thick-gauge pipeline steel. Background Art

[0002] In recent years, the construction of oil and gas pipelines is developing in the direction of large diameter, large wall thickness, and high pressure. It is also facing the test of extreme climate environments such as high cold, swamps, mountains, and seismic activity areas. Faced with such natural environments and geological conditions, how to ensure the safety and stable operation of pipelines is extremely challenging. It can be seen that the key technical requirements of high-grade pipeline steel are to improve the low-temperature toughness index while maintaining high strength. Grain refinement is an effective way to reduce the ductile-brittle transition temperature of steel and improve toughness. For this reason, the organization of high-grade pipeline steel is designed as acicular ferrite, which has a fine microscopic substructure, a fully refined effective grain size, a high proportion of high-angle grain boundaries, and a large dislocation density. It can coordinate and constrain the extension of impact cracks, thereby improving toughness. However, in order to obtain acicular ferrite structure, the coiling temperature of high-grade pipeline steel is low and the cooling rate is large. How to control the stability of the coiling temperature of high-grade pipeline steel under conditions such as large water volume and rapid cooling is a difficult problem in the industrial trial production of high-grade pipeline steel.

[0003] After searching, CN102962296B discloses a low-temperature coiling method for thick-gauge X120 pipeline steel hot-rolled coils, which can effectively improve the plate type, coil shape and coiling stability. The invention optimizes the coiling process in three aspects: the strip is rolled out from the finishing mill and laminar cooled, and the coiling temperature and the strip body temperature within 1m of the strip head are controlled to make the strip head temperature higher than the body temperature; when the strip is laminar cooled, an air blowing device is added to remove the laminar cooling water remaining on the surface of the strip; when coiling, the side guide center line and the side guide opening degree compensation are adjusted and controlled online, the expansion distance of the strip head reel and the opening distance of the auxiliary coiling roller are optimized, and the control of the coiling auxiliary coiling roller is optimized. The invention proposes technologies such as hot head rolling, surface water purge, and side guide alignment for the control of X120 coil type and plate shape, but does not involve how to improve the stability of coiling temperature control when the coiling temperature is low.

[0004] CN105734235B discloses a method for controlling the intensive cooling of hot-rolled strip steel. The cooling equipment on the rolling line is located at the rear side of the finishing mill and the front side of the coiler, including intensive cooling sections, conventional laminar cooling sections and fine-tuning sections, totaling 15 groups of headers. The implementation steps are as follows: after the F1 frame of the finishing mill bites the steel, the cooling model pre-calculates the amount of water required for strip cooling and the number of intensive cooling headers that need to be opened; when the F2 frame of the finishing mill bites the steel, the production control system controls the opening of the cooling model to pre-calculate the intensive cooling headers that need to be opened and the 8 headers in the first half of the 14th group of the fine-tuning section; the hot-rolled mill production control system performs feedback control according to the feedback control calculation results of the cooling model. This invention relates to a laminar cooling intensive cooling model and a header opening method, but does not involve how to improve the coiling temperature control stability when the coiling temperature is low.

[0005] CN105603170B discloses an ultra-fast cooling process and coiling method for ultra-thick hot-rolled coils: 25.4 mm thick X70 strip is rolled out from a finishing mill and cooled to 500-550°C in an ultra-fast cooling section, then air-cooled for 2s, and then cooled to a coiling temperature of 400-450°C in a common layer; the position control time of the pinch roller of the strip head coiler is 0.03s, and the strip is fixed in advance; the number of coiling turns of the strip head is increased to 5 turns, and the auxiliary coiling roller is continuously in contact with the strip head until the reel load torque reaches 12.66KN·M, and the auxiliary coiling roller is opened normally, so that the head is coiled tightly and the strip is close to the tail. The pressure of the auxiliary coiling roller is increased to 750KN to ensure the stable coiling of the tail strip; the tail holding time of the auxiliary coiling roller of the ultra-thick strip tail is 8-12s to fix the shape of the tail strip. This invention aims to solve the problem that 25.4mm thick pipeline steel has high strength and toughness, large springback and is difficult to coil, and proposes key points for controlling the coiling process. However, the coiling temperature of the steel described in this invention is 400-450℃, which is not very low, and this invention does not involve the technology for stabilizing the coiling temperature.

[0006] In summary, there is no report on the control of coiling temperature stability during low-temperature coiling in the patents related to high-grade pipeline steel. Summary of the invention

[0007] The technical problem to be solved by the present invention is that it is difficult to control the temperature stability of high-grade pipeline steel when it is coiled at a relatively low temperature.

[0008] The technical solution adopted by the present invention to solve the technical problem is: a method for stably controlling the low coiling temperature of acicular ferrite thick-gauge pipeline steel: by optimizing the process of finishing rolling and laminar cooling, the coiling temperature of the middle part of the steel coil is stably controlled at 380±20°C for coiling, and the acicular ferrite thick-gauge pipeline steel is prepared, specifically:

[0009] The start rolling temperature of the finishing rolling process is controlled at 910±10℃ and the final rolling temperature is controlled at 795±15℃;

[0010] The laminar cooling process adopts the front-stage centralized cooling and solidified boiling water mode, and divides it into a strong cooling section and a conventional cooling section for cooling by controlling the number of cooling nozzles on the upper and lower headers.

[0011] Furthermore, in the above-mentioned finishing rolling process, when the accumulated deformation is sufficient, the deformation of the finishing rolling final stand is controlled to be 4% to 6%.

[0012] Furthermore, in the above-mentioned finishing rolling process, the rolling speed of the second half of the steel coil is controlled to be greater than the rolling speed of the first half of the steel coil.

[0013] Furthermore, the finishing exit speed of the front half of the steel coil is 2.0m / s to 2.2m / s, and the finishing exit speed of the rear half of the steel coil is 2.2m / s to 2.4m / s.

[0014] Furthermore, in the above laminar cooling process, the upper and lower headers of the 1st to 6th groups are all opened before control; the 1st to 3rd groups of headers are strong cooling sections, and each group of headers is equipped with 16 cooling nozzles; the 3rd to 6th groups of headers are conventional cooling sections, and each group of headers is equipped with 8 cooling nozzles.

[0015] Furthermore, in the above laminar cooling process, the temperature of the laminar cooling water is controlled to be 28°C to 32°C.

[0016] Furthermore, the temperature was measured after the sixth group of headers, and the temperature at the middle point of laminar cooling was found to be 430-470°C.

[0017] Furthermore, in the above laminar cooling process, the water on the surface of the steel plate is completely blown away by controlling the side water spraying; the side water spraying is symmetrically distributed, and the side water spraying surface covers the entire width of the steel plate.

[0018] Furthermore, in the above stable control method, the middle part of the steel coil is the part excluding the head 3m and the tail 3m of the steel coil, and the coiling temperature of the head 3m and the tail 3m of the steel coil is controlled to be 600℃~750℃ during coiling.

[0019] Furthermore, in the above-mentioned stable control method, the acicular ferrite thick-gauge pipeline steel is X80 pipeline steel, whose microstructure is acicular ferrite and the thickness is 15 mm to 25 mm.

[0020] The beneficial effects of the present invention are:

[0021] (1) The present invention aims to solve the problem of low coiling temperature and large amount of laminar cooling water for acicular ferrite pipeline steel, which makes it difficult to stably control laminar cooling. From the perspectives of precise control of rolling temperature, segmented control of rolling speed, and solidification of laminar cooling water model, the present invention systematically solves the problem of stable control of coiling temperature for high-grade pipeline steel.

[0022] (2) Stable control of the high-grade pipeline steel preparation process improves the uniformity of pipeline steel performance, which is beneficial to improving the safety performance of natural gas pipelines. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the coiling temperature of the steel in Example 1;

[0024] Figure 2 is the coiling temperature of the steel in Example 2;

[0025] Figure 3 is the coiling temperature of the steel in Comparative Example 1;

[0026] Figure 4 is the coiling temperature of the steel in Comparative Example 2. DETAILED DESCRIPTION

[0027] The technical solution of the present invention can be specifically implemented in the following manner.

[0028] The reasons for the production process limitations of the acicular ferrite thick-gauge pipeline steel of the present invention are explained below.

[0029] First, in terms of finishing process:

[0030] First, it is required to limit the control accuracy of the finishing rolling entrance temperature and the finishing rolling final rolling temperature. In the present invention, the above temperatures are required to be controlled at 910±10℃ and 795±15℃ respectively. This method is beneficial to improving the temperature uniformity of the steel plate after laminar cooling, that is, improving the control stability of the coiling temperature.

[0031] The finishing rolling entrance temperature is set in the lower temperature range of 900℃~920℃, because at a lower rolling temperature, the steel is deformed in the austenite non-recrystallization zone during the finishing rolling process to form an austenite deformation structure. A large number of original austenite grain boundaries, dislocations, vacancies, etc. accumulated in this process accumulate a large number of nucleation points for the subsequent γ→α phase transformation, promoting grain refinement. When the finishing rolling entrance temperature is too high, it may cause incomplete recrystallization of austenite during the finishing rolling process, forming a mixed crystal structure and reducing the uniformity of the structure.

[0032] The finishing temperature is set in the lower temperature range of 780℃~810℃, in order to promote grain refinement through low temperature and high pressure rolling method, and provide activation energy for the medium temperature phase transformation process of austenite to acicular ferrite. When the finishing temperature is too low, it may cause two-phase rolling in the last few stands after finishing rolling, forming a mixed structure of austenite and ferrite, some structures begin to nucleate, and some structures are still coarse, resulting in reduced uniformity of the structure of the finished steel; when the finishing temperature is too high, it may cause insufficient supercooling during non-recrystallization deformation of austenite, resulting in insufficient refinement of austenite structure during finishing rolling, resulting in coarsening of the finished steel structure, and reducing the strength and toughness of the material.

[0033] Secondly, the finishing process mainly considers the cumulative deformation, because the cumulative deformation determines the degree of flattening of the deformed austenite. High-grade pipeline steel undergoes austenite non-recrystallization zone deformation during the entire finishing rolling process. Under the premise that the cumulative deformation is sufficient, the deformation of the finishing final stand can be appropriately reduced to improve the plate shape of the steel plate and prevent water accumulation on the surface of the steel plate during water cooling. Therefore, the present invention limits the deformation of the finishing final stand to 4% to 6%.

[0034] Finally, when the front half of the intermediate billet is being finish rolled, the back half is in an air-cooled state at the entrance of the finishing mill. In order to improve the uniformity of the coiling temperature along the length of the entire coil, the finishing rolling speed of the back half of the coil is required to be increased from 2.0m / s~2.2m / s to 2.2m / s~2.4m / s.

[0035] Second, in terms of laminar cooling process:

[0036] The present invention requires the use of a front-stage concentrated cooling mode, in which the 1st to 3rd group of headers are strong cooling sections. This is because after finishing rolling, under water cooling conditions, the structure of the steel changes from austenite to ferrite, and acicular ferrite is a bainite structure with a low transformation temperature and a high critical cooling rate. Therefore, the front-stage concentrated rapid cooling is required. At the same time, in order to ensure the stability of the performance of steel coils at different positions and in different batches, the present invention requires the solidification of the laminar cooling water mode, that is, the upper and lower headers of the 1st to 6th groups are all opened, and the temperature of the laminar cooling water is controlled within a stable range, that is, 28°C to 32°C.

[0037] After adopting the above-mentioned solidified laminar cooling model, the midpoint temperature of the steel can be controlled in the range of 430-470°C. The temperature in this temperature range is relatively low, which is conducive to the phase transformation of high-grade pipeline steel during the laminar cooling process of groups 1 to 6 to form acicular ferrite structure.

[0038] In addition, the present invention also requires that the side water spray of the laminar cooling section is symmetrically distributed, and the side water spray sweeping surface covers the full width of the steel plate. This is to ensure that the surface water of the steel plate is completely swept away, otherwise the surface water will quickly heat up under the heat transfer of the steel plate, and the cooling efficiency will quickly decrease. The low-temperature cooling water flowing out of the laminar cooling manifold cannot contact the surface of the steel plate, which will lead to insufficient cooling efficiency of the steel plate, resulting in the inability to form acicular ferrite structure, and the formation of polygonal or equiaxed ferrite, which reduces the strength and toughness of high-grade pipeline steel.

[0039] After adopting the above process, the coiling temperature of most steel coils can be controlled in the temperature range of 380±20°C, which is located in the temperature transformation range of acicular ferrite, which is conducive to the transformation of the steel described in the present invention into acicular ferrite structure.

[0040] The technical solution and effects of the present invention are further illustrated below through practical examples.

[0041] Example

[0042] Example 1

[0043] The process of hot rolling-laminar cooling-coiling was adopted to produce X80 pipeline steel with a thickness of 22.0 mm. The starting rolling temperature was 913°C and the final rolling temperature was 795°C. The finishing rolling exit speed of the first half of the coil was 2.06 m / s and the finishing rolling exit speed of the second half of the coil was 2.33 m / s. The deformation of the last stand of finishing rolling was 4.8%. The laminar cooling water temperature was 31.4°C, the first to sixth groups of headers were all open, the side spray water was all open and symmetrically distributed; the temperature at the middle point of laminar cooling was 458°C.

[0044] After adopting the above process, except for the head and tail of the steel coil which are convenient for coiling due to the hot head and hot tail process (the coiling temperature is 750℃ and 650℃ respectively), the temperature of the rest of the steel coil is in the range of 360℃~400℃, with a narrow fluctuation range of only ±20℃, see attached Figure 1 .

[0045] Example 2

[0046] The process of hot rolling-laminar cooling-coiling was adopted to produce X80 pipeline steel with a thickness of 18.4mm. The starting rolling temperature was 920℃ and the final rolling temperature was 806℃. The finishing rolling exit speed of the first half of the coil was 2.10m / s and the finishing rolling exit speed of the second half of the coil was 2.36m / s. The deformation of the last stand of finishing rolling was 5.8%. The laminar cooling water temperature was 30.8℃, the first to sixth group of headers were all open, the side spray water was all open and symmetrically distributed; the temperature at the middle point of laminar cooling was 461℃.

[0047] After adopting the above process, except for the head and tail of the steel coil, which are convenient for coiling due to the hot head and hot tail process (the coiling temperatures are 750℃ and 650℃ respectively), the temperature of the rest of the steel coil is in the range of 365℃~400℃, with a narrow fluctuation range, see the attached Figure 2 .

[0048] Comparative Example 1

[0049] The process of hot rolling-laminar cooling-coiling was adopted to produce X80 pipeline steel with a thickness of 21.4mm. The starting rolling temperature was 920℃, the final rolling temperature was 806℃; the steel coil finishing exit speed was 1.82m / s; the deformation of the last stand of finishing rolling was 5.4%. The laminar cooling water temperature was 31.4℃, the 1st to 6th group of headers were all opened, the side spray water was all opened and symmetrically distributed; the laminar cooling midpoint temperature was 477℃.

[0050] After adopting the above process, except for the head and tail of the steel coil, the coiling temperature of the first half of the steel coil is 350℃~500℃, and the coiling temperature of the second half of the steel coil is 300~350℃. The temperature of the second half of the steel coil is lower than that of the first half of the steel coil. This is because the finishing rolling exit speed is slow, the temperature drop time of the steel plate in the air is too long, especially the temperature of the second half of the steel coil is low, and the coiling temperature of the whole steel coil fluctuates greatly, with a fluctuation range of 200℃, see attached Figure 3 .

[0051] Comparative Example 2

[0052] The process of hot rolling-laminar cooling-coiling was adopted to produce X80 pipeline steel with a thickness of 15.3mm. The starting rolling temperature was 907℃ and the final rolling temperature was 788℃. The finishing rolling exit speed of the first half of the coil was 2.20m / s and the finishing rolling exit speed of the second half of the coil was 2.40m / s. The deformation of the last stand of finishing rolling was 7.5%. The laminar cooling water temperature was 33.5℃, the first to sixth group of headers were all open, the side spray water was all open and symmetrically distributed; the temperature at the middle point of laminar cooling was 523℃.

[0053] After adopting the above process, due to the high deformation of the last stand of finishing rolling, the plate shape after rolling is poor, and there are edge waves, the side spray water cannot completely collect water on the surface of the steel coil. In addition, the laminar cooling water temperature is high. All these factors lead to the high temperature at the middle point of laminar cooling, the high coiling temperature, and a large fluctuation range of 380℃~510℃. See attached Figure 4 .

Claims

1. A stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel, characterized by: By optimizing the finishing rolling and laminar cooling process, the coiling temperature of the middle part of the steel coil is stably controlled at 380±20℃ for coiling, and the acicular ferrite thick specification pipeline steel is prepared, specifically: The start rolling temperature of the finishing rolling process is controlled at 910±10℃ and the final rolling temperature is controlled at 795±15℃; The laminar cooling process adopts the front-stage centralized cooling and solidified boiling water mode, and divides it into a strong cooling section and a conventional cooling section for cooling by controlling the number of cooling nozzles on the upper and lower headers.

2. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 1, characterized in that: In the finishing process, when the accumulated deformation is sufficient, the deformation of the final stand of the finishing rolling mill is controlled to be 4% to 6%.

3. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 1, characterized in that: In the finishing rolling process, the rolling speed of the second half of the steel coil is controlled to be greater than the rolling speed of the first half of the steel coil.

4. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 3, characterized in that: The finishing exit speed of the first half of the steel coil is 2.0m / s~2.2m / s, and the finishing exit speed of the second half of the steel coil is 2.2m / s~2.4m / s.

5. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 1, characterized in that: In the laminar cooling process, all the upper and lower headers of groups 1 to 6 are opened before control; The first to third groups of headers are strong cooling sections, and each group of headers is equipped with 16 cooling nozzles; The 3rd to 6th groups of headers are conventional cooling sections, and each group of headers is equipped with 8 cooling nozzles.

6. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 1, characterized in that: In the laminar cooling process, the laminar cooling water temperature is controlled to be 28°C to 32°C.

7. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 5, characterized in that: The temperature was measured after the 6th group of headers, and the temperature at the midpoint of laminar cooling was found to be 430-470°C.

8. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 1, characterized in that: In the laminar cooling process, the water on the surface of the steel plate is completely blown away by controlling the side spraying water; The side water sprays are symmetrically distributed, and the side water spray sweeping surface covers the entire width of the steel plate.

9. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 1, characterized in that: The middle part of the steel coil is the part excluding the head 3m and the tail 3m of the steel coil. When coiling, the coiling temperature of the head 3m and the tail 3m of the steel coil is controlled to be 600℃~750℃.

10. The stable control method for low coiling temperature of acicular ferrite thick gauge pipeline steel according to claim 1, characterized in that: The acicular ferrite thick-gauge pipeline steel is X80 pipeline steel, whose microstructure is acicular ferrite and whose thickness is 15 mm to 25 mm.

Citation Information

Patent Citations

  • Production method of X70 hot-rolled medium plate for submerged pipeline

    CN102181796A

  • Pipeline steel X80 coiled plate with super-wide specification and oversized piece weight and production process of coiled plate

    CN103789705A

  • Production method for thick-specification X80 pipeline steel

    CN110656228A

  • Laminar cooling control method for preventing medium-high carbon steel from cracking

    CN112122361A

  • Production method of 550MPa-grade easy-to-form weather-resistant bridge steel

    CN114959469A