Preparation method of fusion welding shaft sleeve of planet shaft of wind power gear box with surface coating
By using copper, tin and nickel alloy materials to weld the steel sleeve surface and spraying self-lubricating materials in wind power gearboxes, the high cost and weight problems of rolling bearings in wind power gearboxes are solved, and the high combination of low-carbon shaft sleeves is achieved Force and fatigue resistance reduce transportation and production costs, and maintain high load-bearing capacity and low wear in oil-free conditions.
Patent Information
- Application Number
- CN202411450666.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-12-03
AI Technical Summary
The high price and weight problems of rolling bearings in wind power gear boxes lead to high manufacturing costs, and traditional sliding bearings are prone to disengage from the bushing under high temperature conditions.
Copper, tin and nickel alloy materials are used to form a coating on the surface of the steel sleeve, and modified polytetrafluoroethylene self-lubricating material is sprayed on the outer surface of the sleeve. The bonding force and fatigue resistance are improved through the welding process and the production cost is reduced. .
The high binding force and fatigue resistance of low-carbon sleeves are achieved, reducing transportation and production costs, while maintaining the high load-bearing capacity and low wear performance of the sleeves under oil-free conditions.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sliding bearing manufacturing, and in particular to a method for preparing a planetary shaft fusion-welded shaft sleeve of a wind power gear box with a surface coating. Background Art
[0002] Rolling bearings have always been used in the planetary shafts of wind power gearboxes to meet the need to reduce friction when the wind blades rotate for a long time. However, the disadvantages of rolling bearings are that they are expensive and have thicker walls, which leads to a heavier overall weight of the gearbox, higher manufacturing costs, and a larger overall volume. Therefore, in order to reduce the manufacturing cost of wind power generation, it is an inevitable trend for sliding bearings to replace rolling bearings. As we all know, sliding bearings are mechanical parts that carry the rotation of the shaft, and they slide and rub against the wear part, so they are called sliding bearings. Generally, sliding bearings are also called sleeves, which is the name of the shape of sliding bearings. In the gearbox of wind power generation, the sliding surface of the sliding bearing is on the outer surface of the sleeve, and the wear part is the inner hole of the gear. Therefore, it has new technical requirements and performance requirements.
[0003] The sliding bearings currently used in wind power generation are copper sleeves directly mounted on the surface of the shaft. Due to the high prices of copper and tin non-ferrous metals, they have lost the advantage of replacing rolling bearings. Therefore, replacing the copper sleeve with a thin copper layer welded on the surface of a steel sleeve is the best choice. Summary of the invention
[0004] In view of this, the present invention provides a method for preparing a wind turbine gearbox planetary shaft fusion-welded sleeve with a surface coating to solve the above-mentioned problem.
[0005] A method for preparing a surface-coated planetary shaft fusion-welded sleeve of a wind power gearbox comprises the following steps: STEP101: Provide a substrate; STEP 102: Provide copper, tin, and nickel alloy materials to prepare the coating, wherein the tin content of the copper, tin, and nickel alloy materials is in the range of 10% to 15%, the nickel content is in the range of 1% to 3%, and the rest is copper; STEP103: Welding the copper, tin and nickel alloy materials onto the substrate by a welding process; STEP104: The sleeve is machined and formed after fusion welding, and after forming, a partial area or the entire area of the outer surface is sprayed with self-lubricating material.
[0006] Furthermore, the substrate is a steel sleeve, and the wall thickness of the steel sleeve is 10 mm to 20 mm.
[0007] Furthermore, the carbon content of the steel sleeve is between 0.1% and 0.5%.
[0008] Furthermore, the thickness of the molten welding alloy is in the range of 0.5 mm to 2 mm.
[0009] Furthermore, the self-lubricating material is modified polytetrafluoroethylene.
[0010] Furthermore, the method for installing the fusion welding bearing on the planetary shaft is to heat the sleeve and then put it on the planetary shaft.
[0011] Compared with the prior art, the preparation method of the planetary shaft fusion-welded sleeve of the wind turbine gearbox with a surface coating provided by the present invention is to weld the alloy material to the surface of the sleeve and then heat-sleeve it on the shaft. Compared with direct fusion welding of copper, tin and nickel alloys on the shaft, 1. The low-carbon sleeve is more likely to meet the requirement of strong welding bonding strength, 2. Reduce the cost of transporting the shaft back and forth, 3. It is easy to carry out surface spraying, and the self-lubricating material can be cured in an ordinary oven to meet the requirements of wind turbines working under oil-free conditions. DETAILED DESCRIPTION
[0012] The specific embodiments of the present invention are further described in detail below. It should be understood that the description of the embodiments of the present invention herein is not intended to limit the protection scope of the present invention.
[0013] The present invention provides a method for preparing a surface-coated wind turbine gearbox planetary shaft fusion-welded sleeve, comprising the following steps: A method for preparing a surface-coated planetary shaft fusion-welded sleeve of a wind power gearbox comprises the following steps: STEP 101 provides a base; STEP 102: Provide copper, tin, and nickel alloy materials to prepare the coating, wherein the tin content of the copper, tin, and nickel alloy materials is in the range of 10% to 15%, the nickel content is in the range of 1% to 3%, and the rest is copper; STEP103: The copper, tin and nickel alloy materials are welded on the substrate by a welding process to form a coating layer; STEP104: The sleeve is machined and formed after fusion welding, and after forming, a partial area or the entire area of the outer surface is sprayed with self-lubricating material.
[0014] Furthermore, the substrate is a steel sleeve, and the wall thickness of the steel sleeve is 10 mm to 20 mm.
[0015] Furthermore, the carbon content of the steel sleeve is between 0.1% and 0.5%.
[0016] Furthermore, the thickness of the molten welding alloy is in the range of 0.5 mm to 2 mm.
[0017] Furthermore, the self-lubricating material is modified polytetrafluoroethylene.
[0018] Furthermore, the method for installing the fusion welding bearing on the planetary shaft is to heat the sleeve and then put it on the planetary shaft.
[0019] In step STEP101, since the fusion-welded sleeve is used for wind power bearings, the required bearing capacity is relatively high, so the matrix is a steel body and has a certain carbon content, which is 0.1% to 0.5%. The wall thickness of the steel sleeve is between 10mm and 20mm, which meets the cutting allowance requirements of the processing process. The surface hardness of low-carbon steel is between HB100 and HB200, and it has strong fatigue resistance. The present invention selects a steel sleeve as the matrix and fusion-welds copper, tin, and nickel alloys on the surface, which not only meets the performance of the original copper sleeve, but also avoids the problem that the sleeve and the shaft are easily moved to the outer ring due to the inconsistent thermal expansion coefficients of copper and steel when the oil temperature rises during operation, and the sleeve is easy to go to the outer ring. At the same time, the production cost is greatly reduced to meet the requirement that the power generation income is higher than the use cost.
[0020] In step STEP102, the self-lubricating material, that is, the copper, tin, and nickel alloy material, is a prior art itself and will not be described in detail here.
[0021] In step STEP103, the coating is mainly used for friction with the steel body in the presence of oil. The coating in the invention is composed of nickel, tin, and copper, and due to the presence of nickel and copper, especially nickel, the fatigue resistance of the self-lubricating material is improved.
[0022] Before preparing the coating by cladding, it is preferred to first lathe the substrate material and the surface to remove the oxide layer and inclusions on the substrate surface. Lathing itself is a prior art and will not be repeated here. The technology for cladding the coating on the substrate is cladding technology, and the cladding methods include laser welding and arc welding. Its purpose is to meet the bonding strength requirements and the alloy layer density, hardness, and performance requirements. In step STEP103, the thickness of the formed coating is between 0.5 mm and 2 mm. If the thickness of the coating is less than 0.5 mm, its wear performance will not meet the service life requirements. If the thickness of the dielectric layer is greater than 2 mm, the strength of the entire coating will be reduced, that is, the bearing capacity of the coating will be reduced.
[0023] In step STEP104, through turning, such as one-time processing of the inside and outside, the wall thickness can be made uniform and the concentricity can be optimal. The coating and the self-coating sprayed on the surface of the coating can withstand high loads and can be free of wear under oil-free and low-speed conditions.
[0024] In some special working conditions, it is not necessary to apply self-lubricating materials. Partial spraying is to save costs. Non-working surfaces can be sprayed without coating, but the positioning during installation needs to be considered to avoid the working surface without spray coating. If the user unit believes that oil lubrication is sufficient, the process of spraying self-lubricating materials on the surface can be cancelled.
[0025] During assembly, the sleeve can be heated in an oven at 100℃~200℃ or in oil to enlarge the inner hole size of the sleeve. After being taken out, it is put on the shaft by its own weight and clamped to the shaft after natural cooling to achieve coaxial fit, meet concentricity requirements and prevent movement during heavy load operation. Example 1
[0026] A method for preparing a surface-coated planetary shaft fusion-welded sleeve of a wind turbine gearbox comprises the following steps: STEP101 provides a substrate, which is a steel sleeve made of low-carbon steel, with a wall thickness of 15 mm and a carbon content of 0.15%. The steel sleeve is a forging; STEP102: After turning, the outer surface is welded with copper, tin and nickel alloy materials, with the tin content in the range of 12%, the nickel content in the range of 2%, and the rest being copper. The alloy can be selected from copper powder or copper wire as the welding base material, preferably to meet the technical requirements; STEP103: The thickness of the fusion welding coating is in the range of 0.8mm. Its thickness is the net thickness after turning, and the fusion welding process needs to leave a processing allowance; STEP104: After the sleeve is machined and formed, a partial or entire outer surface is sprayed with self-lubricating material.
[0027] STEP105: The installation method is to heat the sleeve and then put it on the planetary shaft to bear the friction of the gear or form fluid dynamic pressure between the gears. During installation, the oil holes must be aligned according to the design requirements and installed in place at one time to avoid holding in the middle and failing to assemble to the specified position.
[0028] Compared with the prior art, the preparation method of the planetary shaft fusion-welded sleeve of the wind turbine gearbox with a surface coating provided by the present invention is to weld the alloy material to the surface of the sleeve and then heat-sleeve it on the shaft. Compared with direct fusion welding of copper, tin and nickel alloys on the shaft, 1. The low-carbon sleeve is more likely to meet the requirement of strong welding bonding strength, 2. Reduce the cost of transporting the shaft back and forth, 3. It is easy to carry out surface spraying, and the self-lubricating material can be cured in an ordinary oven to meet the requirements of wind turbines working under oil-free conditions.
[0029] The above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modification, equivalent substitution or improvement within the spirit of the present invention is included in the scope of the claims of the present invention.
Claims
1. A method for preparing a surface-coated planetary shaft fusion-welded sleeve of a wind turbine gearbox, comprising the following steps: STEP101: Provide a substrate; STEP 102: Provide copper, tin, and nickel alloy materials to prepare the coating, wherein the tin content of the copper, tin, and nickel alloy materials is in the range of 10% to 15%, the nickel content is in the range of 1% to 3%, and the rest is copper; STEP103: welding the copper, tin and nickel alloy materials onto the substrate through a welding process to form the coating; STEP104: The sleeve is machined and formed after fusion welding, and after forming, a partial area or the entire area of the outer surface is sprayed with self-lubricating material.
2. The method for preparing the surface-coated planetary shaft fusion-welded sleeve of a wind turbine gearbox according to claim 1, Features: The substrate is a steel sleeve with a wall thickness of 10 mm to 20 mm.
3. The method for preparing the surface-coated wind turbine gearbox planetary shaft fusion-welded sleeve according to claim 2, Features: The carbon content of the steel sleeve is between 0.1% and 0.5%.
4. The method for preparing the surface-coated wind turbine gearbox planetary shaft fusion-welded sleeve according to claim 1, Features: The thickness of the fusion welding alloy is in the range of 0.5mm to 2mm.
5. The method for preparing the surface-coated wind turbine gearbox planetary shaft fusion-welded sleeve according to claim 1, Features: The self-lubricating material is modified polytetrafluoroethylene.
6. The method for preparing the surface-coated planetary shaft fusion-welded sleeve of a wind turbine gearbox according to claim 1, Features: The method for installing the fusion-welded bearing to the planetary shaft is to heat the sleeve and then put it on the planetary shaft.
Citation Information
Patent Citations
Steel-based composite copper axle bush and manufacturing method thereof
CN110144490A
Wind turbine gearbox and method for producing a wind turbine gearbox
CN111936756A
Preparation method of fusion welding shaft sleeve with surface lubricating layer for planet shaft of wind power gear box