Preparation method of anti-reflection light trapping glass and application of anti-reflection light trapping glass in solar cell
The preparation of plasma structures with oxide shell wrapped in metal cores through self-assembly technology has solved the problems of high cost and low cost performance of the existing plasma trap light-enhancing structure, and achieved a low-cost trap light-enhancing effect, suitable for solar energy Batteries and photovoltaic equipment.
Patent Information
- Application Number
- CN202310642382.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
AI Technical Summary
The existing plasma trap light-enhancing structure is costly and the direct contact between metal and semiconductors leads to composite losses, which is not cost-effective and has no practical industrial cases, especially in perovskite solar cells.
Self-assembly technology is used to prepare plasma structures with oxide shells wrapped in metal cores. By changing the film thickness, composition and laser scanning parameters of the metal film, the plasma array structure is regulated to achieve a light-enhancing effect and avoid direct contact between metal and semiconductors. Reduce costs.
It realizes a low-cost light enhancement effect, improves the transmittance and absorption capacity of photovoltaic equipment, has commercial potential, and is suitable for solar cells and other photovoltaic applications.
Smart Images

Figure CN119059740A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation of anti-reflection light-trapping glass. A film layer with plasma anti-reflection light-trapping characteristics of a micro-nano structure is prepared on a glass surface with a metal film deposited thereon by laser ablation, thereby achieving a light-trapping anti-reflection effect. The present invention specifically relates to a light-trapping anti-reflection glass, a preparation method and photovoltaic applications thereof. Background Art
[0002] Currently, the world's annual photovoltaic installed capacity has exceeded 300GW and is still growing rapidly. Even with the current installed capacity, for every 1% increase in light transmission or absorption, assuming 20% of it is converted into solar power, the new installed capacity can generate an additional 1 million kilowatt-hours of solar power per hour.
[0003] Plasma light trapping and anti-reflection structures are rarely used in the production of solar cells. Take perovskite as an example. Perovskite cells have become the hottest research and development and manufacturing fields due to their excellent carrier mobility, insensitivity to grain boundaries, and high absorption rate. Due to the rapid nucleation and growth of perovskite crystals and the fast preparation process, the light absorption layer crystals themselves have many light trapping structures such as cavities and rough surface interface morphology. Therefore, there are not many studies on light trapping and anti-reflection for this type of battery. Plasma light trapping and anti-reflection structures are usually not cheap, and because there will be recombination losses and self-absorption losses when metals and semiconductors are in direct contact, the cost performance is not high, so there has been no industrial practical case so far.
[0004] The present invention uses self-assembly technology to prepare a plasma structure in which an oxide shell wraps a metal core, which has a significant transmittance enhancement and light trapping effect. In addition, since the oxide shell separates the direct contact between the metal and the semiconductor and there is no related recombination; and since the metal core is small, the absorption loss can be ignored. Laser ablation self-assembly technology has low cost and commercial potential. Summary of the invention
[0005] The present invention provides a light-trapping glass with enhanced transmittance, a preparation method and its application in photovoltaics. The plasma array structure is regulated by changing the film thickness, composition, laser scanning parameters and the like of a metal film, thereby achieving the purpose of light-trapping with enhanced transmittance.
[0006] To achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows: The present invention provides a method for preparing anti-reflection light-trapping glass, comprising the following steps: (1) Depositing a metal film on glass; (2) Laser scanning the glass surface after the metal film is deposited in step (1) to form a micro-nano structure plasma array on the glass surface to obtain a transmittance-enhancing light-trapping glass.
[0007] Furthermore, the metal film includes at least one of a nickel film, a molybdenum film, an iron film, a titanium film, a copper film, a vanadium film, a copper film, an alloy film, etc.; and the deposition thickness of the film is 50 nm-2000 nm.
[0008] Preferably, the deposition thickness of the inorganic thin film is 100 nm to 1000 nm.
[0009] Furthermore, the deposition method includes magnetron sputtering, electron beam evaporation, thermal evaporation, and electroplating.
[0010] Furthermore, when the deposition method is magnetron sputtering, the typical settings are: DC sputtering of a water-cooled Ni target with a diameter of 60 mm, the sputtering gas is pure Ar, the working gas pressure is 1.6 Pa, the argon gas flow rate is 30 sccm, the ignition voltage is 350 V, the sputtering voltage is 290 V-300 V, the current is 0.180 A-0.190 A, and the deposition time is 10 min.
[0011] Furthermore, the deposition rate is adjusted by adjusting the working gas pressure, argon gas flow rate, sputtering voltage, and current to achieve the target deposition thickness; the deposition rate is 0.01 Å / s to 1000 Å / s.
[0012] In the present invention, different equipment has different process parameters, which can be selected according to actual needs.
[0013] Furthermore, the deposition method is to add other target deposition materials such as high-purity nickel particles into a graphite crucible during electron beam evaporation, and manually adjust the electron beam spot size, with a typical deposition rate of 0.1 Å / s to 500 Å / s, until the target thickness is deposited.
[0014] Furthermore, the laser light source for the laser scanning is at least one of a solid-state laser light source, a gas phase laser light source, a fiber laser light source, an infrared laser light source, an ultraviolet laser light source, and a visible light laser light source.
[0015] Furthermore, the rated power of the laser is 0.3W-10000W.
[0016] Furthermore, the wavelength of the laser light source is 20 nm-100 µm.
[0017] Preferably, the laser scanning uses a 30W rated power fiber laser with a wavelength of 1064 nm. Furthermore, the laser energy density should be greater than 30 mJ / cm 2 , scanning speed is 0.01 m / s-100 m / s; scanning line spacing ≤50mm; Preferably, the laser energy density is about 76 J / cm 2, the scanning speed is 0.5 m / s-3 m / s; the scanning line spacing is 0.03 mm.
[0018] Furthermore, the glass includes solar cell cover glass, ITO conductive glass for thin-film batteries, soda-lime glass, borosilicate glass, tempered glass, aluminosilicate glass, quartz glass, automotive glass, architectural glass, etc. Furthermore, the anti-reflection light-trapping glass is only used as the inner surface of solar cells. It can also be used as a substrate for photovoltaic windows, thin-film cells and stacked solar cells, and further deposition of ITO, electron transport layer, perovskite absorption layer, hole transport layer, etc. on it does not change the original process path for producing perovskite cells.
[0019] Compared with the prior art, the advantages and beneficial effects of the present invention are: 1. The present invention uses low-cost laser ablation self-assembly technology to achieve the effect of light trapping and light enhancement, which is superior to the existing technology. Moreover, the present invention is applied to the inner surface to avoid the requirements for mechanical properties such as wear resistance of the film layer; the plasma light trapping and light enhancement effect is better when applied to the high dielectric absorption layer.
[0020] 2. In terms of technology, the deposition method of the present invention uses magnetron sputtering; the requirements for laser scanning are low, and a fiber laser marker or an ultraviolet laser marker can meet the requirements; the entire preparation method is low-cost and can be completed using industrially stable and mature equipment, and has the advantage of scalable production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a photo of the laser-treated nickel glass and the control glass after the SnS light-absorbing layer was deposited in Example 1.
[0022] Figure 2 It is a transmittance diagram of the laser-treated nickel glass and the control glass after the SnS light absorbing layer is deposited in Example 1.
[0023] Figure 3 It is a transmittance diagram of the laser-treated nickel glass and the control glass after SnS solar cell devices were deposited in Example 1. The SnS solar cell device comprises a TiO2 electron transport layer, a light absorption layer, a NiO hole transport layer and a nickel-aluminum metal electrode.
[0024] Figure 4 These are typical scanning electron microscope (SEM) photos of the glass surface after treatment in Example 1 and electron energy spectrum (EDS) mapping pictures.
[0025] Figure 5 It is the transmittance diagram of the treated glass and the control glass in Example 2.
[0026] Figure 6It is the transmittance diagram of the treated glass and the control glass in Example 3.
[0027] Figure 7 is the transmittance of the glass after treatment in Example 4.
[0028] Figure 8 These are typical scanning electron microscope (SEM) photos of the glass surface after treatment in Example 4 and electron energy spectrum (EDS) mapping pictures.
[0029] Fig. 9 This is a SEM image of the glass surface after treatment in Example 3. Implementation
[0030] The following embodiments are used to better illustrate the present invention, but the present invention is not limited to the following embodiments. Example
[0031] The specific steps of preparing anti-reflection light-trapping glass using nickel film and its application in thin-film SnS batteries are as follows: (1) Deposition of nickel film by magnetron sputtering coating system: the back vacuum is 10 -4 Pa level, DC sputtering of water-cooled nickel target (99.995%) with a diameter of 60 mm, sputtering gas is pure Ar (99.9995%), working pressure is 1.6 Pa; substrate is 1.5 mm thick soda lime glass or conductive ITO glass; argon gas flow rate is 30 sccm, ignition voltage is 350V, sputtering voltage is 290 V-300 V, current is 0.180A-0.190 A, deposition time is 10min. The thickness of the deposited film is about 350 nm as detected by laser confocal microscopy.
[0032] Laser scanning the glass surface after the nickel film is deposited in step (1), forming a micro-nano structure composed of nickel-based core-shell structure nanoparticles on the glass surface; using a fiber laser marking machine with a rated power of 30W for laser scanning; the laser scanning conditions are: 100% power corresponds to approximately 76J / cm 2 Energy density; scanning speed 2 m / s; scanning line spacing 0.02 mm; frequency 30 kHz; transmission enhanced glass was obtained.
[0033] A SnS light absorbing layer and a SnS thin film battery are deposited on the anti-reflection glass and the control glass, respectively. The SnS light absorbing layer deposition process is as follows. The base pressure is 2.1×10 -6 Pa, SnS evaporation temperature is maintained at 675℃, substrate temperature is maintained at 375℃, and deposition time is 20min. SnS thin film battery deposition also includes titanium oxide electron transport layer of about 100nm, nickel oxide hole transport layer of about 20nm and nickel aluminum electrode of about 1.5µm.
[0034] Figure 1 The following are photos of laser-treated nickel glass and control glass after SnS light-absorbing layer was deposited. Obvious transmission enhancement can be seen. The laser-treated nickel glass after SnS light-absorbing layer was deposited can still see a clear background, while the control glass cannot see the background clearly. This shows that the light-trapping glass prepared by the present invention is more suitable for use in photovoltaic windows. Figure 2 The transmittance comparison chart of laser-treated nickel glass and control glass after depositing SnS light-absorbing layer is shown. It can be seen that the transmittance of laser-treated nickel glass is much higher than that of control glass, and the transmittance in the visible light band is increased by about 15%. Figure 3 The transmittance comparison chart of laser-treated nickel glass and control glass deposited with SnS devices is shown. There is a significant increase in transmittance in the visible and infrared light fields, with an increase of nearly 10% in the visible light band and an even more significant increase of 15% in the infrared band. This kind of transmittance enhancement is crucial for photovoltaic windows; for opaque cells, it can further improve their absorption of sunlight, which is equivalent to all the transmission in this embodiment being completely absorbed by the opaque perovskite cell or silicon cell; for stacked cells, the absorption enhancement in the infrared band will also be more significant. Figure 4 a shows the SEM image of the laser-treated nickel glass surface, showing that the surface is composed of fine dispersed nanoparticles. Figure 4 b shows Figure 4 The EDS mapping result of sample a shows that the nanoparticles are a core-shell structure with a metal core wrapped in oxide. Because laser ablation is carried out in air, these nanoparticles should be the result of the melt condensed and crystallized on the surface, and severe oxidation is inevitable in this process. Therefore, these nanoparticles are a structure of a nickel core wrapped in an oxide shell. The above excellent anti-reflection effect is caused by the plasma polarization and scattering effect corresponding to this core-shell nanostructure. Example
[0035] The specific steps of magnetron sputtering molybdenum film to prepare anti-reflection light-trapping glass are as follows: (1) Molybdenum film was deposited by magnetron sputtering system. A water-cooled Mo target with a diameter of 60 mm was sputtered by DC sputtering. The sputtering gas was pure Ar, the working pressure was 1.6 Pa, the Ar flow rate was 30 sccm, the ignition voltage was 260 V, the sputtering voltage was 270 V-280 V, the current was 0.880 A-0.900 A, and the deposition time was 10 min. The thickness of the deposited film was about 450 nm as detected by confocal microscopy.
[0036] Laser scanning the glass surface after the molybdenum film is deposited in the step (1), forming a micro-nano structure on the glass surface; using a fiber laser marking machine with a rated power of 30W for laser scanning; the laser scanning conditions are: 30W power; scanning speed 2m / s; scanning spacing 0.02mm; frequency 30khz; to obtain transmission enhanced glass. Figure 5It shows that the anti-reflection glass has an enhanced transmission of more than 0.5% in the visible light band compared to the control glass, and the control glass is the 100% reference line in the figure. Example
[0037] The specific steps of the preparation method of the anti-reflection light-trapping glass based on tungsten film are as follows: (1) Deposit tungsten film on glass using a magnetron sputtering coating system: the backing vacuum is 10 -4 Pa level; DC sputtering of water-cooled tungsten target (99.95%) with a diameter of 60 mm, sputtering gas is pure Ar (99.9995%), working pressure is 1.6 Pa, argon flow rate is set to 30 sccm; ignition voltage is 300V, sputtering voltage is 280 V-290 V, current is 0.24A-0.3 A, coating makes the voltage unstable, need to be manually adjusted to maintain the power at about 70W, deposition time is 5min. The film thickness is about 100nm.
[0038] (2) Laser scanning: The glass surface after the tungsten film is deposited in step (1) is marked by a fiber laser marking machine with a power of 27 W, a scanning speed of 2 m / s, and a scanning line spacing of 0.03 mm; thus, a light-trapping anti-reflection glass is obtained. Figure 6 It shows that the anti-reflection glass has an enhanced transmission of more than 0.5% in the visible light band compared to the control glass, and the control glass is the 100% reference line in the figure. Example
[0039] The titanium film is used to prepare the anti-reflection light-trapping glass. The specific steps are as follows: (1) The back vacuum is 10 -4 Pa level; DC sputtering of a water-cooled titanium target (99.95%) with a diameter of 60 mm, the sputtering gas is pure Ar (99.9995%), the working gas pressure is 1.6 Pa, and the argon flow rate is set to 30 sccm; the sputtering power is manually adjusted to maintain about 60 W, and the deposition time is 5 min.
[0040] (2) Laser scanning: After the titanium film is deposited in step (1), a micro-nano structure is formed on the glass surface; a fiber laser marking machine with a rated power of 30W is used for laser scanning; the laser scanning conditions are: 21W power; scanning speed 2m / s; scanning interval 0.02mm; frequency 30khz; and the light-trapping glass with enhanced transmittance is obtained. Figure 7 It can be seen that the transmittance in the visible light band is enhanced by about 1%. Figure 8 a shows the SEM photo of the laser-treated titanium glass surface, showing that the surface is composed of fine dispersed nanoparticles. Figure 8 b shows Figure 8The EDS mapping result of sample a shows that the nanoparticles have a core-shell structure with a titanium core wrapped in oxide. Most of the nanoparticles have been oxidized. The excellent anti-reflection effect is caused by the plasma polarization and scattering effect corresponding to this core-shell nanostructure. Example
[0041] The specific steps of the preparation method of the anti-reflection light-trapping glass based on the copper alloy (copper-nickel-aluminum) film are as follows: (1) Using magnetron sputtering system to deposit copper-aluminum-nickel alloy film on glass: back vacuum to 10 -4 Pa level; strong magnetic and weak magnetic targets were used to DC sputter a 60 mm diameter water-cooled copper target (99.9995%), and a 60 mm diameter water-cooled aluminum target (99.9995%), and a 60 mm diameter water-cooled nickel target (99.9995%) was sputtered simultaneously with RF; the sputtering gas was pure Ar (99.9995%), the working pressure was 1.6 Pa; the argon gas flow rate was set to 30 sccm. Copper sputtering was a strong magnetic target sputtering, the sputtering voltage and current were 300V-0.51A respectively; RF sputtering nickel power was 80W; aluminum sputtering was a weak magnetic target sputtering, the sputtering voltage and current were 270V-0.05A respectively. The three targets sputtered at the same time and ended at the same time, and the co-deposition time was 5 min.
[0042] (2) Laser scanning The glass surface after the copper-nickel alloy film is deposited in step (1) is scanned by a 30W fiber laser with 100% power, a scanning speed of 1.5m / s, and a scanning line spacing of 0.03mm to obtain a light-trapping anti-reflection glass. The effect is shown in Fig. 9 , the transmittance in the visible light band is increased by about 0.5%, and the reference glass is the 100% reference line in the figure.
[0043] As shown in the above embodiments, the transmittance-enhancing and light-trapping properties of the glass can be adjusted by adjusting the composition and thickness of the thin film material and the laser scanning parameters. The transmittance-enhancing and light-trapping effects of the glass can be more significant when applied to solar cells as the inner surface of their cover glass or as their substrates. Therefore, the main application of the present invention is solar glass. The deposition rate can be adjusted by adjusting the gas pressure, argon gas flow rate, sputtering voltage, and current in the thin film deposition process. It is only necessary to reach the target deposition thickness of the film. The glass performance can also be changed by adjusting the power, scanning speed and other parameters in the laser scanning process. Therefore, it has the advantage of large-scale production. The glass obtained by the above preparation method of the present invention can also be used in windows of integrated solar cells, substrates of thin-film solar cells, substrates of laminated solar cells, and other glasses that require transmittance-enhancing and light-trapping properties. The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.
Claims
1. A method for preparing anti-reflection light-trapping glass, characterized in that: The following steps are involved: (1) depositing a metal film on the glass (the metal may be at least one of nickel, molybdenum, iron, tungsten, titanium, vanadium, copper, etc. or an alloy thereof); (2) Laser scanning the glass surface after the thin film deposition in step (1) to obtain the anti-reflection light-trapping glass.
2. The method for preparing the anti-reflection light-trapping glass according to claim 1, characterized in that: The glass includes solar cell cover glass, ITO conductive glass for thin film batteries, soda-lime glass, borosilicate glass, tempered glass, aluminosilicate glass, quartz glass, automotive glass, architectural glass, etc.
3. The method for preparing the anti-reflection light-trapping glass according to claim 1, characterized in that: The deposition thickness of the metal film is 50 nm-2000 nm.
4. The method for preparing the anti-reflection light-trapping glass according to claim 1, characterized in that: The laser light source for the laser scanning is at least one of a solid-state laser light source, a gas phase laser light source, a fiber laser light source, an infrared laser light source, an ultraviolet laser light source, and a visible light laser light source.
5. The method for preparing anti-reflection light-trapping glass according to claim 1, characterized in that: The laser scanning energy density should be greater than 30 mJ / cm 2 .
6. The glass according to claim 1, if it is not ITO conductive glass, the prepared anti-reflection light-trapping glass can be used as the inner surface of solar cells; it can also be used as the substrate of thin-film solar cells and stacked solar cells, and the ITO, electron transport layer, perovskite absorption layer, hole transport layer, etc. are further deposited thereon without changing the original process path for producing perovskite cells.
7. If the glass according to claim 1 is ITO conductive glass, the prepared anti-reflection light-trapping glass can be used as the inner surface of solar cells; it can also be used as the substrate of thin-film cells and stacked solar cells, and further deposition of ITO layer, electron transport layer, perovskite absorption layer, hole transport layer, etc. on it does not change other process paths for producing perovskite cells. It is just that in some cases, the ITO layer can be omitted.
8. The anti-reflection light-trapping glass prepared by the preparation method according to any one of claims 1 to 7, the preparation method and the application of the glass in solar cells.