Antibacterial glass cover plate and preparation method thereof
By forming an Ag/TiO2/SiO2 composite layer on the surface of the glass cover, the problem of bacteria accumulation and cleaning of the glass cover after long-term use is solved, and efficient antibacterial effect is achieved. It is suitable for surface cleaning of mobile phones and other mobile terminals .
Patent Information
- Application Number
- CN202411181573.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Glass covers are prone to accumulate bacteria after long-term use and are not easy to clean. The prior art lacks effective solutions.
The nanoporous glass surface was formed by wet chemical acid etching, and then an aminolated TiO2/SiO2 composite coating was prepared on the glass surface, and an Ag/TiO2/SiO2 composite layer was formed by complexing silver ions in the silver precursor solution to achieve silver Uniform adsorption and binding of nanoparticles.
The formed Ag/TiO2/SiO2 composite layer generates superoxide radicals under light irradiation, effectively killing bacteria, SiO2 enhances the binding force with glass, ensuring long-term antibacterial performance, silver nanoparticles significantly improve the antibacterial effect, effectively clearing mobile phones Bacteria in the surface and decorative ring grooves.
Smart Images

Figure BDA0005012318240000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass processing, and in particular relates to an antibacterial glass cover plate and a preparation method thereof. Background Art
[0002] The development of mobile communication technology has changed people's work and lifestyle, and mobile terminals such as mobile phones have become an indispensable part of people's daily lives.
[0003] As an important part of mobile phones, the glass cover plate is in direct contact with users for the longest time every day, so it is extremely easy to accumulate bacteria and other substances, which have a certain impact on the health of users. Therefore, in order to keep it clean, users must use alcohol to wipe the glass cover plate of the mobile phone to effectively remove the bacteria on it. However, for ordinary users, there is little special alcohol to regularly clean the glass cover plate of the mobile phone. In addition, due to the special structure of the mobile phone, it is very inconvenient to effectively clean the dirt or bacteria accumulated around the mobile phone. Summary of the invention
[0004] Based on the above technical problems, the present invention provides an antibacterial glass cover plate and a preparation method thereof, which effectively solves the problem that the glass cover plate is prone to accumulate bacteria and difficult to clean after long-term use by in-situ modification on the surface of the glass cover plate to form an Ag / TiO2 / SiO2 composite layer.
[0005] The present invention provides a method for preparing an antibacterial glass cover, comprising the following steps:
[0006] S1, performing wet chemical acid etching on the glass cover plate to obtain a glass cover plate having nanopores on the surface;
[0007] S2, immersing the glass cover plate having nanopores on the surface into an amino TiO2 / SiO2 mixed sol, and after curing, obtaining a glass cover plate having an amino TiO2 / SiO2 composite coating on the surface;
[0008] S3, immersing the glass cover plate having the TiO2 / SiO2 composite coating on the surface into a silver precursor solution, and after heat treatment, obtaining a glass cover plate having the Ag / TiO2 / SiO2 composite coating on the surface, which is the antibacterial glass cover plate.
[0009] In the present invention, nanopores are formed on the surface of the glass cover plate by wet chemical acid etching, so as to obtain a glass cover plate surface with high surface energy; then, an amination TiO2 / SiO2 composite system sol is prepared by a sol-gel method, so as to prepare an amination TiO2 / SiO2 composite coating tightly bonded to the surface of the glass cover plate, and then the glass cover plate is immersed in a silver precursor solution. Since the amination TiO2 / SiO2 composite coating formed on the surface of the glass cover plate has amino groups, the amino TiO2 / SiO2 composite coating can form a complex with silver ions in the silver precursor solution, so that the silver ions can be uniformly and effectively adsorbed and bonded on the surface of the glass cover plate, and then the silver particles are reduced to form nanometer-level silver particles, so as to obtain an Ag / TiO2 / SiO2 composite coating that can be uniformly dispersed and effectively bonded to the surface of the glass cover plate.
[0010] Preferably, in step S1, the wet chemical acid etching specifically comprises: immersing the glass cover plate in an acid etching solution for etching, wherein the acid etching solution comprises, by weight percentage, HF 0.01-0.5wt%, H2SO4
[0011] 0.01-0.1wt%, HNO30.01-0.1wt%, HCl 0.01-0.1wt%, H2SiO30.1-1wt%, and the balance is deionized water.
[0012] Preferably, the temperature of the wet chemical acid etching is 40-80° C. and the time is 12-36 hours.
[0013] Preferably, in step S2, the amino TiO2 / SiO2 mixed sol is prepared by dissolving titanate, silicate and aminosilane coupling agent in an alcohol solvent and acidifying and hydrolyzing them;
[0014] Preferably, the titanate is n-propyl titanate or n-butyl titanate, the silicate is ethyl orthosilicate, propyl orthosilicate or butyl orthosilicate, the aminosilane coupling agent is 3-aminopropyltrimethoxysilane or 3-(2-aminoethylamino)propyltrimethoxysilane, and the alcohol solvent is methanol, ethanol, propanol or butanol;
[0015] Preferably, the molar ratio of the titanate, silicate and aminosilane coupling agent is 1:0.3-0.5:0.1-0.3.
[0016] Preferably, in step S2, the curing comprises: heating to 80-120°C, keeping warm for 0.5-2h, heating to 150-200°C, keeping warm for 0.5-2h, heating to 250-300°C, keeping warm for 0.5-2h.
[0017] Preferably, in step S3, the silver precursor solution comprises, by weight percentage: 1-5wt% silver nitrate, 5-10wt% sodium citrate, and the balance is deionized water.
[0018] Preferably, in step S3, the heat treatment temperature is 130-180° C. and the time is 1-3 h.
[0019] Preferably, the glass cover is made of ordinary soda-lime-silica glass, aluminosilicate glass or borosilicate glass.
[0020] The present invention also provides an antibacterial glass cover plate, which is prepared by the above preparation method.
[0021] Preferably, the antibacterial glass cover plate comprises a glass cover plate substrate and an Ag / TiO2 / SiO2 composite layer located on the surface of the glass cover plate substrate.
[0022] Beneficial effects: In the present invention, a Ag / TiO2 / SiO2 composite coating is formed on the surface of the glass cover plate. Firstly, the nanoparticle layer of TiO2 can generate superoxide free radicals under light irradiation, which can kill bacteria efficiently and quickly; secondly, the nanoparticle layer of SiO2 and the nanoparticle layer of TiO2 are combined to form a synergistic effect, and SiO2 can strengthen the bonding force between the nanoparticle layer of TiO2 and the glass cover plate, ensuring that the glass cover plate obtains long-term antibacterial performance; the silver nanoparticle layer has a more obvious bactericidal effect, which can further improve the antibacterial effect; finally, when the glass cover plate of the present invention is applied to the surface of a mobile terminal such as a mobile phone, it can effectively remove bacteria and other harmful substances on the surface of the mobile phone and in the grooves of the surrounding decorative rings, thereby solving the problem that the current mobile phone is prone to accumulate bacteria and is difficult to clean after long-term use. DETAILED DESCRIPTION
[0023] Hereinafter, the present invention will describe the technical solution in detail through specific embodiments, but it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0024] Example 1
[0025] This embodiment provides an antibacterial glass cover plate, and the preparation method thereof includes:
[0026] (1) A glass cover substrate (soda-lime-silica glass) with a thickness of 1.2 mm was placed in ultrapure water, acetone, and ethanol for ultrasonic cleaning for 30 min respectively, and then dried with nitrogen gas; then immersed in an acid etching solution, wherein the acid etching solution includes, by weight percentage, HF 0.1wt%, H2SO4 0.04wt%, HNO3 0.05wt%, HCl 0.06wt%, H2SiO3 0.5wt%, and the balance is deionized water, and etched at 60° C. for 24 h, and then washed with ultrapure water and dried with nitrogen gas to obtain a glass cover substrate with nanopores on the surface;
[0027] (2) Tetrabutyl titanate, tetraethyl orthosilicate and 3-aminopropyltrimethoxysilane are added to anhydrous ethanol in a molar ratio of 1:0.4:0.2 and dissolved completely, and then an aqueous nitric acid solution is added, the amount of nitric acid used is 1.5 times the molar amount of tetrabutyl titanate, the temperature is raised to 60°C, and the reaction is stirred for 4 hours to obtain a clear and stable amino TiO2 / SiO2 mixed sol; the glass cover plate with nanopores on the surface is immersed in the amino TiO2 / SiO2 mixed sol, and then pulled out at a uniform speed with a pulling instrument, and the temperature is raised to 100°C, kept warm for 1 hour, raised to 180°C, kept warm for 1 hour, and raised to 280°C, kept warm for 1 hour to obtain a glass cover plate with an amino TiO2 / SiO2 composite coating on the surface;
[0028] (3) Immersing the glass cover plate having an amino TiO2 / SiO2 composite coating on the surface into a silver precursor solution for 10 minutes, wherein the silver precursor solution comprises: 2wt% silver nitrate, 7wt% sodium citrate, and the balance is deionized water. After taking out, the solution is kept warm at 150°C for 2h to obtain a glass cover plate having an Ag / TiO2 / SiO2 composite coating on the surface, which is the antibacterial glass cover plate.
[0029] Example 2
[0030] This embodiment provides an antibacterial glass cover plate, and the preparation method thereof includes:
[0031] (1) A glass cover substrate (soda-lime-silica glass) with a thickness of 1.2 mm was placed in ultrapure water, acetone, and ethanol for ultrasonic cleaning for 30 min respectively, and then dried with nitrogen gas; then immersed in an acid etching solution, wherein the acid etching solution comprises, by weight percentage, HF 0.03 wt%, H2SO4 0.09 wt%, HNO3 0.02 wt%, HCl 0.1 wt%, H2SiO3 0.1 wt%, and the balance is deionized water, and etched at 40° C. for 36 h, and then washed with ultrapure water and dried with nitrogen gas to obtain a glass cover substrate with nanopores on the surface;
[0032] (2) Tetrabutyl titanate, ethyl orthosilicate and 3-(2-aminoethylamino)propyltrimethoxysilane are added to anhydrous ethanol in a molar ratio of 1:0.3:0.3 to dissolve completely, and then an aqueous nitric acid solution is added, wherein the amount of nitric acid used is 1.5 times the molar amount of tetrabutyl titanate, the temperature is raised to 60°C, and the reaction is stirred for 4 hours to obtain a clear and stable amino TiO2 / SiO2 mixed sol; the glass cover plate having nanopores on the surface is immersed in the amino TiO2 / SiO2 mixed sol, and then pulled out at a uniform speed with a pulling instrument, and the temperature is raised to 80°C, kept warm for 2 hours, then raised to 150°C, kept warm for 2 hours, and then raised to 250°C, kept warm for 2 hours to obtain a glass cover plate having an amino TiO2 / SiO2 composite coating on the surface;
[0033] (3) Immersing the glass cover plate having an amino TiO2 / SiO2 composite coating on the surface into a silver precursor solution for 10 minutes, wherein the silver precursor solution comprises: 1wt% silver nitrate, 5wt% sodium citrate, and the balance is deionized water. After taking out, the solution is kept warm at 130°C for 3 hours to obtain a glass cover plate having an Ag / TiO2 / SiO2 composite coating on the surface, which is the antibacterial glass cover plate.
[0034] Example 3
[0035] This embodiment provides an antibacterial glass cover plate, and the preparation method thereof includes:
[0036] (1) A glass cover substrate (soda-lime-silica glass) with a thickness of 1.2 mm was placed in ultrapure water, acetone, and ethanol for ultrasonic cleaning for 30 min respectively, and then dried with nitrogen gas; then immersed in an acid etching solution, wherein the acid etching solution includes, by weight percentage, HF 0.5wt%, H2SO4 0.01wt%, HNO3 0.09wt%, HCl 0.02wt%, H2SiO3 0.9wt%, and the balance is deionized water, and etched at 60° C. for 24 h, and then washed with ultrapure water and dried with nitrogen gas to obtain a glass cover substrate with nanopores on the surface;
[0037] (2) Tetrabutyl titanate, tetraethyl orthosilicate and 3-aminopropyltrimethoxysilane are added to anhydrous ethanol in a molar ratio of 1:0.5:0.1 and dissolved completely, and then an aqueous nitric acid solution is added, the amount of nitric acid used is 1.5 times the molar amount of tetrabutyl titanate, the temperature is raised to 60°C, and the reaction is stirred for 4 hours to obtain a clear and stable amino TiO2 / SiO2 mixed sol; the glass cover plate with nanopores on the surface is immersed in the amino TiO2 / SiO2 mixed sol, and then pulled out at a uniform speed with a pulling instrument, and the temperature is raised to 120°C, kept warm for 0.5h, raised to 200°C, kept warm for 0.5h, raised to 300°C, and kept warm for 0.5h to obtain a glass cover plate with an amino TiO2 / SiO2 composite coating on the surface;
[0038] (3) Immersing the glass cover plate having an amino TiO2 / SiO2 composite coating on the surface into a silver precursor solution for 10 minutes, wherein the silver precursor solution comprises: 5wt% silver nitrate, 10wt% sodium citrate, and the balance is deionized water. After taking out, the solution is kept warm at 180°C for 1 hour to obtain a glass cover plate having an Ag / TiO2 / SiO2 composite coating on the surface, which is the antibacterial glass cover plate.
[0039] Comparative Example 1
[0040] This comparative example proposes an antibacterial glass cover plate, and the preparation method thereof comprises:
[0041] (1) A glass cover substrate (soda-lime-silica glass) with a thickness of 1.2 mm was placed in ultrapure water, acetone, and ethanol for ultrasonic cleaning for 30 min respectively, and then dried with nitrogen gas; then immersed in an acid etching solution, wherein the acid etching solution includes, by weight percentage, HF 0.1wt%, H2SO4 0.04wt%, HNO3 0.05wt%, HCl 0.06wt%, H2SiO3 0.5wt%, and the balance is deionized water, and etched at 60° C. for 24 h, and then washed with ultrapure water and dried with nitrogen gas to obtain a glass cover substrate with nanopores on the surface;
[0042] (2) Tetrabutyl titanate and 3-aminopropyltrimethoxysilane are added to anhydrous ethanol at a molar ratio of 1:0.2 and dissolved completely, and then an aqueous nitric acid solution is added, the amount of nitric acid used is 1.5 times the molar amount of tetrabutyl titanate, the temperature is raised to 60°C, and the reaction is stirred for 4 hours to obtain a clear and stable amino TiO2 sol; the glass cover plate with nanopores on the surface is immersed in the amino TiO2 sol, and then pulled out at a uniform speed with a pulling instrument, and the temperature is raised to 100°C, kept warm for 1 hour, raised to 180°C, kept warm for 1 hour, and raised to 280°C, kept warm for 1 hour to obtain a glass cover plate with an amino TiO2 coating on the surface;
[0043] (3) Immersing the glass cover plate having an amino TiO2 coating on the surface into a silver precursor solution for 10 minutes, wherein the silver precursor solution comprises: 2wt% silver nitrate, 7wt% sodium citrate, and the balance is deionized water. After taking out, the solution is kept warm at 150°C for 2 hours to obtain a glass cover plate having an Ag / TiO2 composite coating on the surface, namely the antibacterial glass cover plate.
[0044] Comparative Example 2
[0045] This comparative example proposes an antibacterial glass cover plate, and the preparation method thereof comprises:
[0046] (1) A glass cover substrate (soda-lime-silica glass) with a thickness of 1.2 mm was placed in ultrapure water, acetone, and ethanol for ultrasonic cleaning for 30 min respectively, and then dried with nitrogen gas; then immersed in an acid etching solution, wherein the acid etching solution includes, by weight percentage, HF 0.1wt%, H2SO4 0.04wt%, HNO3 0.05wt%, HCl 0.06wt%, H2SiO3 0.5wt%, and the balance is deionized water, and etched at 60° C. for 24 h, and then washed with ultrapure water and dried with nitrogen gas to obtain a glass cover substrate with nanopores on the surface;
[0047] (2) Tetrabutyl titanate and ethyl orthosilicate are added to anhydrous ethanol at a molar ratio of 1:0.4 and dissolved completely, and then an aqueous nitric acid solution is added, wherein the amount of nitric acid used is 1.5 times the molar amount of tetrabutyl titanate, the temperature is raised to 60°C, and the reaction is stirred for 4 hours to obtain a clear and stable TiO2 / SiO2 mixed sol; the glass cover plate having nanopores on the surface is immersed in the TiO2 / SiO2 mixed sol, and then pulled out at a uniform speed using a pulling instrument, and the temperature is raised to 100°C, kept warm for 1 hour, raised to 180°C, kept warm for 1 hour, and raised to 280°C, kept warm for 1 hour to obtain a glass cover plate having a TiO2 / SiO2 composite coating on the surface;
[0048] (3) Immersing the glass cover plate having a TiO2 / SiO2 composite coating on the surface into a silver precursor solution for 10 minutes, wherein the silver precursor solution comprises: 2wt% silver nitrate, 7wt% sodium citrate, and the balance is deionized water. After taking out, the solution is kept warm at 150°C for 2 hours to obtain a glass cover plate having a Ag / TiO2 / SiO2 composite coating on the surface, which is the antibacterial glass cover plate.
[0049] The antibacterial performance test of the antibacterial glass cover plate of the embodiment and the comparative example refers to the standard "JC / T 897-2002 Antibacterial Performance of Antibacterial Ceramic Products", and the two bacterial species of Escherichia coli and Staphylococcus aureus are tested; the test environment conditions are temperature 25°C, relative humidity 75%, and natural light; the results are shown in Table 1 below:
[0050] Table 1 Antibacterial properties of the antibacterial glass cover plates described in Examples and Comparative Examples
[0051]
[0052] The above table shows that the antibacterial rate of the glass cover plate treated by the present invention against Staphylococcus aureus and Escherichia coli is significantly increased compared with the glass cover plate not treated by the present invention, and the general antibacterial rate is more than 20% higher; and compared with the glass cover plate in which the SiO2 nanoparticle coating modification is omitted (Comparative Example 1), or the glass cover plate without amino modification (Comparative Example 2), the antibacterial rate of the glass cover plate of the embodiment is significantly improved, and its antibacterial performance is the best.
[0053] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing an antibacterial glass cover, characterized in that: The steps include: S1, performing wet chemical acid etching on the glass cover plate to obtain a glass cover plate having nanopores on the surface; S2, immersing the glass cover plate having nanopores on the surface into an amino TiO2 / SiO2 mixed sol, and after curing, obtaining a glass cover plate having an amino TiO2 / SiO2 composite coating on the surface; S3, immersing the glass cover plate having the TiO2 / SiO2 composite coating on the surface into a silver precursor solution, and after heat treatment, obtaining a glass cover plate having the Ag / TiO2 / SiO2 composite coating on the surface, which is the antibacterial glass cover plate.
2. The method for preparing the antibacterial glass cover according to claim 1, characterized in that: In step S1, the wet chemical acid etching specifically includes: immersing the glass cover plate in an acid etching solution for etching, wherein the acid etching solution includes, by weight percentage: HF 0.01-0.5wt%, H2SO4 0.01-0.1wt%, HNO3 0.01-0.1wt%, HCl 0.01-0.1wt%, H2SiO3 0.1-1wt%, and the balance is deionized water.
3. The method for preparing the antibacterial glass cover according to claim 2, characterized in that: The temperature of the wet chemical acid etching is 40-80° C. and the time is 12-36 hours.
4. The method for preparing the antibacterial glass cover according to any one of claims 1 to 3, characterized in that: In step S2, the amino TiO2 / SiO2 mixed sol is prepared by dissolving titanate, silicate and aminosilane coupling agent in an alcohol solvent and then acidifying and hydrolyzing them; Preferably, the titanate is n-propyl titanate or n-butyl titanate, the silicate is ethyl orthosilicate, propyl orthosilicate or butyl orthosilicate, the aminosilane coupling agent is 3-aminopropyltrimethoxysilane or 3-(2-aminoethylamino)propyltrimethoxysilane, and the alcohol solvent is methanol, ethanol, propanol or butanol; Preferably, the molar ratio of the titanate, silicate and aminosilane coupling agent is 1:0.3-0.5:0.1-0.
3.
5. The method for preparing the antibacterial glass cover according to any one of claims 1 to 4, characterized in that: In step S2, the curing includes: heating to 80-120°C, keeping warm for 0.5-2h, heating to 150-200°C, keeping warm for 0.5-2h, heating to 250-300°C, keeping warm for 0.5-2h.
6. The method for preparing the antibacterial glass cover according to any one of claims 1 to 5, characterized in that: In step S3, the silver precursor solution comprises, by weight percentage, 1-5 wt % silver nitrate, 5-10 wt % sodium citrate, and the balance is deionized water.
7. The method for preparing the antibacterial glass cover according to any one of claims 1 to 6, characterized in that: In step S3, the heat treatment temperature is 130-180° C. and the time is 1-3 hours.
8. The method for preparing the antibacterial glass cover according to any one of claims 1 to 7, characterized in that: The glass cover plate is made of common soda-lime-silica glass, aluminosilicate glass or borosilicate glass.
9. An antibacterial glass cover, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 8.
10. The antibacterial glass cover plate according to claim 9, characterized in that: It comprises a glass cover substrate and an Ag / TiO2 / SiO2 composite layer located on the surface of the glass cover substrate.
Citation Information
Patent Citations
Antireflection coated glass with self-cleaning effect and preparation method thereof
CN102838288A
Preparation method of anti-reflection self-cleaning coated glass
CN103086613A
Preparation method of ultra-hydrophilic transparent SiO2 / TiO2 antifog film
CN103771721A
Self-cleaning coating with enhanced light transmittance
CN108948802A
Preparation method of AF coated glass with antibacterial effect
CN112456812A
Cited By
Antibacterial medicinal glass bottle and preparation method thereof
CN121913713A