Recycled concrete micro-powder modification method based on process control

By using surfactant and Bacillus assisted carbonization process control method in recycled concrete powder, the problem of recycled concrete powder after carbonization in the prior art is solved, efficient modification and energy saving are achieved, and concrete is improved mechanical properties.

CN119059753APending Publication Date: 2024-12-03HOHAI UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410839631.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing recycled concrete micropowder modification technology, filtration and drying are required after carbonization, resulting in large energy consumption and cumbersome process, and the utilization rate of micropowder is not high.

Method used

Using a process-controlled method, the regenerated concrete micropowder is placed in the nanosilicon dioxide & nanotitanium dioxide suspension of the surfactant vanillin-based polyoxyethylene ether, and the carbonization is assisted by Bacillus to reduce the regenerated concrete micropowder after carbonization. the reprocessing step improves its mechanical strength and activity.

Benefits of technology

The modification process without suction filtration and drying greatly reduces energy losses and improves the mechanical properties and activity of recycled concrete powder. As an auxiliary cementitious material, it can partially replace cement and enhance the mechanical properties of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059753A_ABST
    Figure CN119059753A_ABST
Patent Text Reader

Abstract

The invention discloses a recycled concrete micro-powder modification method based on process control. The method comprises the following steps: pretreating recycled concrete micro-powder by using a silane coupling agent KH550, so that the KH550 is adsorbed on the surface of the recycled concrete micro-powder; the nano titanium dioxide suspension is used as a medium for modifying the recycled concrete micro powder, so that the surface of the recycled concrete micro powder is coated with the nano titanium dioxide suspension, gas containing carbon dioxide is continuously introduced into the nano titanium dioxide suspension for wet carbonization, and meanwhile, bacillus is used for assisting in improving the carbonization effect. By controlling the modification process of the recycled concrete micro-powder, the steps of suction filtration, drying and the like of the concrete micro-powder are optimized, the energy consumption in the process is reduced, the micro-powder with relatively fine particles is reserved, and the carbonization efficiency is improved by nano suspension and bacillus. The recycled concrete micropowder carbonized through process control has better pozzolanic activity, and can be used as a high-quality supplementary cementing material to replace cement to be doped into a concrete material. According to the process control-based mixed carbonization method provided by the invention, the energy consumption in the traditional carbonization process is reduced, the carbonization efficiency can be greatly improved, and the purposes of carbon reduction and carbon sequestration of resource utilization of the recycled concrete micro powder are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a recycled concrete fine powder modification method based on process control. Background Art

[0002] In recent decades, the construction industry has developed rapidly, especially in developing countries, resulting in the depletion of natural resources and the generation of large amounts of construction and demolition waste. The rapid expansion of my country's economy has led to the gradual replacement of old buildings with modern structures. As a result, the demolition of these abandoned buildings has led to the accumulation of a large amount of waste concrete. The effective utilization of waste concrete has important practical significance for achieving sustainable social development and protecting the ecological environment.

[0003] The use of recycled concrete powder as an auxiliary cementitious material to replace part of cement has been promoted as a way to effectively utilize construction waste and save natural resources. However, compared with concrete made from pure cement, concrete mixed with recycled concrete powder still has problems such as poor mechanical properties and durability. Recycled concrete powder accounts for 20%-30% of the production of recycled concrete aggregate. Chinese patent CN113185229A discloses a green high-performance recycled concrete and its preparation method, mentioning that the powder generated in the process of producing recycled concrete aggregate enters the pores of the recycled concrete aggregate from the surface for filling. However, this technology uses unhydrated cement, and specifically removes the hydrated powder, and teaches that the removal of the hydrated powder is conducive to the later filling of the pores by calcium carbonate. This causes a waste of recycled powder and a waste of resources spent on the early processing of powder, and it is impossible to make full use of recycled materials and energy.

[0004] The main components of recycled concrete are similar to cement, but recycled concrete powder contains less calcium oxide but more silica, alumina, ferrous oxide and magnesium oxide. In addition, the alkali content in recycled concrete powder is higher than that in cement, while the sulfate content in recycled concrete powder is lower than that in cement. Recently, some studies have shown that carbonated recycled concrete powder exhibits better mechanical properties and pozzolanic reactivity. CO2 can react rapidly with cement hydration products such as Ca(OH)2 and CSH gel under humid conditions, and can completely carbonize the powder in cement hydration paste within a few hours. This means that recycled concrete powder may completely undergo carbonation reaction in aqueous solution in a short period of time to produce products such as calcium carbonate and silica gel.

[0005] In the existing recycled concrete powder modification process, filtration and drying are usually required, which greatly increases the energy consumption in the modification process and is inconsistent with the original intention of using recycled concrete powder. For example, Chinese patent CN112125541A discloses a method for wet carbonization activation of waste concrete recycled powder, and the modification method is: the powder produced in the process of crushing waste concrete to produce recycled aggregate is used as recycled powder, the recycled powder is dispersed in water to form a mixed slurry, industrial waste gas containing carbon dioxide is continuously introduced into the mixed slurry, and the mixed slurry after the carbonization reaction is completed is filtered and dried to obtain high-activity recycled powder, which can be used as an auxiliary cementitious material. In this patent, the recycled concrete powder is subjected to wet carbonization treatment, but it needs to be filtered and dried after treatment, and the carbonization method is single, and the utilization rate of the powder is not high.

[0006] Therefore, how to control the process of modified recycled concrete powder to obtain modified recycled concrete powder with excellent performance is a current technical challenge. Summary of the invention

[0007] In order to overcome the problem that the existing wet modification process of recycled concrete micropowder requires filtering and drying the recycled concrete micropowder after carbonization, resulting in high energy consumption, cumbersome process, time-consuming and labor-intensive process, the present invention proposes a modification method based on process control without reprocessing the recycled concrete micropowder after carbonization. The method places the recycled concrete micropowder in a nano-silicon dioxide & nano-titanium dioxide suspension to which a surfactant vanillin polyoxyethylene ether (VAEO8) is added for carbonization, and simultaneously adopts Bacillus to assist carbonization and continuously introduces carbon dioxide to improve the mechanical strength and activity of the recycled concrete micropowder, and introduces nano-silicon dioxide and nano-titanium dioxide as auxiliary materials. The obtained modified recycled concrete micropowder composition can partially replace cement as an auxiliary cementitious material, and is mixed with mineral aggregate to form concrete.

[0008] At the same time, the present invention examines the reaction parameters that achieve the best experimental effect in the above reaction process, that is, the experimental parameters that can maximize the mechanical strength of the recycled concrete powder, including the powder particle size, the concentration of the KH550 ethanol solution, the percentage of the suspension of nano-silicon dioxide & nano-titanium dioxide, the temperature of each step and the reaction time.

[0009] In view of the defects existing in the prior art, the present invention aims to achieve the above objectives. The technical solution adopted by the present invention includes:

[0010] A method for modifying recycled concrete powder based on process control, characterized in that it comprises the following raw materials: recycled concrete powder, silane coupling agent KH550, nano silicon dioxide, nano titanium dioxide, surfactant, Bacillus KW, sucrose, deionized water, and gas containing carbon dioxide;

[0011] The method comprises the following steps implemented in sequence:

[0012] 1) Grinding waste concrete to a target particle size to obtain recycled concrete powder;

[0013] 2) Adsorbing silane coupling agent KH550 on the surface of recycled concrete powder;

[0014] 3) drying the micro powder and cooling;

[0015] 4) preparing a suspension of nano-silicon dioxide and nano-titanium dioxide containing a surfactant, wherein the total mass of the nano-silicon dioxide and nano-titanium dioxide accounts for 1-3% of the mass of the recycled concrete micropowder; mixing the recycled concrete micropowder cooled in step 3) with the nano-silicon dioxide and nano-titanium dioxide suspension to prepare a mixed slurry;

[0016] 5) Add 1-2 g / L sucrose to the prepared Bacillus solution for cultivation; the Bacillus powder accounts for 1%-3% of the mass of the recycled concrete powder;

[0017] 6) Pour the mixed slurry and the Bacillus solution into a reactor, heat the reactor in a water bath at 20-25° C., stir during heating, and introduce a gas containing carbon dioxide into the reactor at a rate of 1-3 L / min during stirring to ensure that the pressure in the reactor is 0.2-0.3 MPa. The reaction process lasts for 1-3 hours.

[0018] Preferably, the particle size of the recycled concrete powder satisfies D90=45 μm, that is, among all particles of the recycled concrete powder, particles with a particle size greater than 45 μm account for 10%, and particles with a particle size less than 45 μm account for 90%.

[0019] Preferably, the silane coupling agent KH550 is in the form of a solution, which is prepared by adding 10-15% of KH550 to an ethanol solution and fully hydrolyzing it; the content of the ethanol solution is ethanol:water=2:1-3:1.

[0020] Preferably, the nano-silicon dioxide and the nano-titanium dioxide are simultaneously present in a nano-silicon dioxide & nano-titanium dioxide suspension, and the nano-silicon dioxide & nano-titanium dioxide suspension is prepared by mixing hydrophilic gas-phase nano-silicon dioxide and nano-titanium dioxide powder with deionized water and then ultrasonically dispersing them for 10-30 minutes; the average particle size range of the nano-silicon dioxide & nano-titanium dioxide in the suspension is 15-20nm.

[0021] Preferably, a surfactant vanillin polyoxyethylene ether (VAEO8) of the same mass as the nanomaterial is added to the nano-silicon dioxide & nano-titanium dioxide suspension, and magnetic stirring is performed at a speed of 100-200 r / min for 15-30 min to ensure uniform dispersion of the nano-silicon dioxide and nano-titanium dioxide in the suspension.

[0022] Preferably, the Bacillus KW is prepared by weighing 1-3% bacterial powder to prepare a microbial solution. After the solution is prepared, 1-2 g / L of sucrose is added thereto, and the solution is placed in a constant temperature shaker and shaken for 15-20 hours at a speed of 150-200 r / min and a temperature of 25-30°C.

[0023] Preferably, the modified recycled concrete powder is included in the water-cement ratio as a solid as an auxiliary cementitious material, and the nano-silicon dioxide & nano-titanium dioxide suspension is included in the water-cement ratio as a liquid.

[0024] Preferably, the method comprises the following steps:

[0025] Step S1: crushing the collected waste concrete test blocks with a jaw crusher, and then grinding the broken blocks with a particle size greater than 4.75 mm with a ball mill again, and sieving the products to obtain recycled concrete powder, with a controlled particle size of 0.02-0.045 mm;

[0026] Step S2: adding 10-15% KH550 to an ethanol solution to fully hydrolyze it, wherein the ethanol solution is ethanol:water=2:1-3:1, to obtain a KH550 ethanol solution; then, adding the obtained recycled concrete powder to the above solution, heating it to 60-85°C, and magnetically stirring it at a speed of 100-200 r / min for 1-2 hours to allow KH550 to be adsorbed on the surface of the recycled powder;

[0027] Step S3: placing the recycled concrete powder obtained in step S2 in a constant temperature oven at 100-120° C., drying until the mass is constant, then taking it out and cooling it to room temperature;

[0028] Step S4: preparing a suspension of nano-silicon dioxide & nano-titanium dioxide containing a surfactant, wherein the total mass of the nano-silicon dioxide & nano-titanium dioxide accounts for 1-3% of the mass of the recycled concrete powder; mixing the recycled concrete powder cooled in step S3 with the nano-silicon dioxide & nano-titanium dioxide suspension to prepare a mixed slurry;

[0029] Step S5: treating the mixed slurry at a power of 500-700 W for 1-3 min, and then treating it again at the same power for 1-3 min after an interval of 1-2 min to make it preliminarily evenly dispersed;

[0030] Step S6: weighing the Bacillus powder according to the ratio of 1-3% of the mass of the recycled concrete powder to prepare a microbial solution, and after the solution is prepared, adding 1-2g / L of sucrose thereto, placing it in a constant temperature shaker, and shaking and culturing it at a speed of 150-200r / min and a temperature of 25-30°C for 15-20h;

[0031] Step S7: Pour the mixed slurry after microwave-assisted dispersion in step S5 and the microbial solution into a reactor, heat the reactor in a water bath at 20-25°C, and magnetically stir the recycled concrete powder and nano-silicon dioxide & nano-titanium dioxide suspension in the reactor at a speed of 200-300r / min during the heating process, and introduce carbon dioxide-containing gas into the reactor at a rate of 1-3L / min during the stirring process to ensure that the pressure in the reactor is 0.2-0.3MPa, and continue carbonization for 0.1-3h.

[0032] Preferably, the ball mill grinding in step S1 is preferably a planetary ball mill with a rotation speed of 300-400 r / min, a grinding time of 8-10 min, and a ball-to-material ratio of 4:1-8:1.

[0033] Preferably, in step S2, the preferred mass ratio of recycled concrete powder to KH550 ethanol solution is 1:10.

[0034] Preferably, the chemical composition of the recycled concrete powder meets the following requirements: SiO2 content is 35-42%, CaO content is 34-40%

[0035] Preferably, in step S3, the preferred drying temperature is 100-120° C., and the drying time is 7-9 hours.

[0036] Preferably, the nano-silicon dioxide & nano-titanium dioxide suspension in step S4 preferably uses vanillin polyoxyethylene ether (VAEO8) with the same total amount as the nano-silicon dioxide & nano-titanium dioxide as a surfactant.

[0037] Preferably, in step S4, the nano silicon dioxide and nano titanium dioxide have the same mass.

[0038] The present invention also provides modified recycled concrete fine powder obtained according to the modification method.

[0039] The present invention also provides an application of the wet modified recycled concrete powder based on process control in cement paste, wherein the recycled concrete powder modified by the above method replaces cement at a replacement rate of 40%.

[0040] The invention provides a method for modifying recycled concrete micropowder based on process control. The recycled concrete micropowder is immersed in a nano-silicon dioxide & nano-titanium dioxide suspension to which a surfactant vanillin-based polyoxyethylene ether (VAEO8) is added, and the suspension is placed in a reaction kettle for heating and stirring in a water bath, and a gas containing carbon dioxide (with a purity of >99%) is continuously introduced into the reaction kettle. In the presence of Bacillus, during this process, nano-silicon dioxide & nano-titanium dioxide are coated on the surface of the recycled concrete micropowder and fill the pores inside the recycled concrete micropowder, and the carbon dioxide reacts with the recycled concrete micropowder.

[0041] Beneficial effects of the present invention:

[0042] 1. The present invention uses nano-silicon dioxide and nano-titanium dioxide suspensions as wet carbonization media. Nano-silicon dioxide and nano-titanium dioxide both play auxiliary roles, enhance the effect of surface modification of recycled concrete powder, further improve the activity of recycled concrete powder, provide more nucleation sites for the formation of CSH, and make the interface transition zone near the recycled concrete powder more compact, thereby improving the mechanical properties of the clean slurry.

[0043] 2. The present invention uses Bacillus KW to assist carbonization during wet carbonization. Bacillus KW adapts to high alkaline environments and will not cause harm to the human body and the environment. Its special enzymatic hydrolysis characteristics can promote the conversion of CO2 to HCO3-. Under alkaline conditions, HCO3- reacts with OH- to generate CO32-, which reacts with cations such as Ca2+ in a continuous chelating environment to generate carbonates, further repairing the defects of the recycled aggregate.

[0044] 3. The present invention does not require filtration and drying after modifying the recycled concrete powder, which greatly reduces energy loss and saves time, and ensures the activity of the recycled concrete powder preserved in the form of a suspension.

[0045] 4. The present invention examines the reaction parameters that achieve the best experimental effect in the above reaction process, that is, the experimental parameters that can maximize the mechanical strength of the recycled concrete powder, including the powder particle size, the concentration of the KH550 ethanol solution, the percentage of the suspension of nano-silicon dioxide & nano-titanium dioxide, the temperature of each step and the reaction time.

[0046] 5. The recycled concrete powder carbonized by process control in the present invention has good volcanic ash activity and can be added to concrete materials as a high-quality supplementary cementitious material to replace cement.

[0047] After the recycled concrete powder is modified, the proportion of the recycled concrete powder as an auxiliary cementitious material can be increased while ensuring the strength, thereby promoting the use of the recycled concrete powder. The mixed carbonization method based on process control provided by the present invention not only reduces the energy consumption in the traditional carbonization process, but also greatly improves the carbonization efficiency, thereby achieving the carbon reduction and carbon fixation goals of the resource utilization of recycled concrete powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 Schematic diagram of the process of recycled concrete powder modification.

[0049] Figure 2 It is a graph of the compressive strength of the embodiments and the comparative examples. DETAILED DESCRIPTION

[0050] The present invention is further described below in conjunction with the examples, and those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the disclosure disclosed herein. This application is intended to cover any modifications, uses or adaptations of the present invention, which follow the general principles of the present invention and include common knowledge or customary technical means in the art that are not disclosed in the present invention.

[0051] Example 1

[0052] (1) The collected waste concrete test blocks were crushed with a jaw crusher and sieved. Then, the broken blocks with a particle size greater than 4.75 mm were ground again with a planetary ball mill at a speed of 300 r / min for 8 min with a ball-to-material ratio of 6:1. The product was sieved through a 325-mesh sieve to obtain recycled concrete powder with a particle size of 0.045 mm.

[0053] (2) 15% KH550 was added dropwise to an ethanol solution having a volume ratio of ethanol to water of 2:1 to prepare a KH550 ethanol solution. The regenerated micropowder was weighed and mixed with the KH550 ethanol solution at a mass ratio of 1:10, heated to 80 degrees Celsius, and continuously stirred with a magnetic force at a speed of 200 r / min for 8 minutes.

[0054] (3) Weigh 2 parts of Bacillus powder and 10 parts of distilled water to prepare a microbial solution at room temperature. After the solution is prepared, add 0.1 parts of sucrose and place it in a constant temperature shaker for shaking and incubation at a speed of 200 r / min and a temperature of 25°C for 20 h.

[0055] (4) At room temperature, 2 parts of gas-phase nano-silica, 2 parts of nano-titanium dioxide powder, 4 parts of vanillin polyoxyethylene ether (VAEO8) and 35 parts of distilled water were weighed and added into a beaker. The mixture was stirred magnetically for 20 minutes to prepare a nano-silica & nano-titanium dioxide suspension. 40 parts of modified recycled concrete powder were weighed and mixed with the nano-silica & nano-titanium dioxide suspension to form a mixed slurry. The mixed slurry was subjected to microwave treatment at a power of 600 W for 3 minutes. After an interval of 2 minutes, the mixed slurry was subjected to microwave treatment at the same power for 3 minutes.

[0056] (5) The microwave-treated mixed slurry and the microbial solution were added to the reactor, the water temperature was maintained at 25°C, the rotation speed was 200 r / min, and CO2-containing gas (purity>99%) was introduced into the reactor at a rate of 2 L / min, and the reaction was continued for 2 h.

[0057] (6) The mixed slurry after carbonization in (5) was mixed with 60 parts of ordinary Portland cement and added into a stirrer. The mixture was slowly stirred at a speed of 150 r / min for 1 min and then quickly stirred at a speed of 400 r / min for 2 min to obtain a cement slurry. The slurry was poured into a mold and vibrated to form a dense shape. The slurry was demolded after 1 day. After standard curing for 28 days, the compressive strength of the test block obtained after curing was tested according to GB / T 17671-1999 Cement mortar strength test method (ISO method).

[0058] Example 2

[0059] (1) The collected waste concrete test blocks were crushed with a jaw crusher and sieved. Then, the broken blocks with a particle size greater than 4.75 mm were ground again with a planetary ball mill at a speed of 300 r / min for 8 min with a ball-to-material ratio of 6:1. The product was sieved through a 325-mesh sieve to obtain recycled concrete powder with a particle size of 0.045 mm.

[0060] (2) 15% KH550 was added dropwise to an ethanol solution having a volume ratio of ethanol to water of 2:1 to prepare a KH550 ethanol solution. The regenerated micropowder was weighed and mixed with the KH550 ethanol solution at a mass ratio of 1:10, heated to 80 degrees Celsius, and continuously stirred with a magnetic force at a speed of 200 r / min for 8 minutes.

[0061] (3) Weigh 2 parts of Bacillus powder and 10 parts of distilled water to prepare a microbial solution at room temperature. After the solution is prepared, add 0.1 parts of sucrose and place it in a constant temperature shaker for shaking and incubation at a speed of 200 r / min and a temperature of 25°C for 20 h.

[0062] (4) At room temperature, 4 parts of gas-phase nano-silica, 4 parts of nano-titanium dioxide powder, 8 parts of vanillin polyoxyethylene ether (VAEO8) and 35 parts of distilled water were weighed and added into a beaker. The mixture was stirred magnetically for 20 minutes to prepare a nano-silica & nano-titanium dioxide suspension. 40 parts of modified recycled concrete powder were weighed and mixed with the nano-silica & nano-titanium dioxide suspension to form a mixed slurry. The mixed slurry was subjected to microwave treatment at a power of 600 W for 3 minutes. After an interval of 2 minutes, the mixed slurry was subjected to microwave treatment at the same power for 3 minutes.

[0063] (5) The microwave-treated mixed slurry and the microbial solution were added to the reactor, the water temperature was maintained at 25°C, the rotation speed was 200 r / min, and CO2-containing gas (purity>99%) was introduced into the reactor at a rate of 2 L / min, and the reaction was continued for 2 h.

[0064] (6) The mixed slurry after carbonization in (5) was mixed with 60 parts of ordinary Portland cement and added into a stirrer. The mixture was slowly stirred at a speed of 150 r / min for 1 min and then quickly stirred at a speed of 400 r / min for 2 min to obtain a cement slurry. The slurry was poured into a mold and vibrated to form a dense shape. The slurry was demolded after 1 day. After standard curing for 28 days, the compressive strength of the test block obtained after curing was tested according to GB / T 17671-1999 Cement mortar strength test method (ISO method).

[0065] Example 3

[0066] (1) The collected waste concrete test blocks were crushed with a jaw crusher and sieved. Then, the broken blocks with a particle size greater than 4.75 mm were ground again with a planetary ball mill at a speed of 300 r / min for 8 min with a ball-to-material ratio of 6:1. The product was sieved through a 325-mesh sieve to obtain recycled concrete powder with a particle size of 0.045 mm.

[0067] (2) 15% KH550 was added dropwise to an ethanol solution having a volume ratio of ethanol to water of 2:1 to prepare a KH550 ethanol solution. The regenerated micropowder was weighed and mixed with the KH550 ethanol solution at a mass ratio of 1:10, heated to 80 degrees Celsius, and continuously stirred with a magnetic force at a speed of 200 r / min for 8 minutes.

[0068] (3) Weigh 2 parts of Bacillus powder and 10 parts of distilled water to prepare a microbial solution at room temperature. After the solution is prepared, add 0.1 parts of sucrose and place it in a constant temperature shaker for shaking and incubation at a speed of 200 r / min and a temperature of 25°C for 20 h.

[0069] (4) At room temperature, 6 parts of gas-phase nano-silica, 6 parts of nano-titanium dioxide powder, 12 parts of vanillin polyoxyethylene ether (VAEO8) and 45 parts of distilled water were weighed and added into a beaker. The mixture was stirred magnetically for 20 minutes to prepare a nano-silica & nano-titanium dioxide suspension. 40 parts of modified recycled concrete powder were weighed and mixed with the nano-silica & nano-titanium dioxide suspension to form a mixed slurry. The mixed slurry was subjected to microwave treatment at a power of 600 W for 3 minutes. After an interval of 2 minutes, the mixed slurry was subjected to microwave treatment at the same power for 3 minutes.

[0070] (5) The microwave-treated mixed slurry and the microbial solution were added to the reactor, the water temperature was maintained at 25°C, the rotation speed was 200 r / min, and CO2-containing gas (purity>99%) was introduced into the reactor at a rate of 2 L / min, and the reaction was continued for 2 h.

[0071] (6) The mixed slurry after carbonization in (5) was mixed with 60 parts of ordinary Portland cement and added into a stirrer. The mixture was slowly stirred at a speed of 150 r / min for 1 min and then quickly stirred at a speed of 400 r / min for 2 min to obtain a cement slurry. The slurry was poured into a mold and vibrated to form a dense shape. The slurry was demolded after 1 day. After standard curing for 28 days, the compressive strength of the test block obtained after curing was tested according to GB / T 17671-1999 Cement mortar strength test method (ISO method).

[0072] Example 4

[0073] (1) The collected waste concrete test blocks were crushed with a jaw crusher and sieved. Then, the broken blocks with a particle size greater than 4.75 mm were ground again with a planetary ball mill at a speed of 300 r / min for 8 min with a ball-to-material ratio of 6:1. The product was sieved through a 325-mesh sieve to obtain recycled concrete powder with a particle size of 0.045 mm.

[0074] (2) 15% KH550 was added dropwise to an ethanol solution having a volume ratio of ethanol to water of 2:1 to prepare a KH550 ethanol solution. The regenerated micropowder was weighed and mixed with the KH550 ethanol solution at a mass ratio of 1:10, heated to 80 degrees Celsius, and continuously stirred with a magnetic force at a speed of 200 r / min for 8 minutes.

[0075] (3) Weigh 2 parts of Bacillus powder and 10 parts of distilled water to prepare a microbial solution at room temperature. After the solution is prepared, add 0.1 parts of sucrose and place it in a constant temperature shaker for shaking and incubation at a speed of 200 r / min and a temperature of 25°C for 20 h.

[0076] (4) At room temperature, 4 parts of gas-phase nano-silica, 4 parts of nano-titanium dioxide powder, 8 parts of vanillin polyoxyethylene ether (VAEO8) and 35 parts of distilled water were weighed and added into a beaker. The mixture was stirred magnetically for 20 minutes to prepare a nano-silica & nano-titanium dioxide suspension. 40 parts of modified recycled concrete powder were weighed and mixed with the nano-silica & nano-titanium dioxide suspension to form a mixed slurry. The mixed slurry was subjected to microwave treatment at a power of 600 W for 3 minutes. After an interval of 2 minutes, the mixed slurry was subjected to microwave treatment at the same power for 3 minutes.

[0077] (5) The microwave-treated mixed slurry and the microbial solution were added to the reactor, the water temperature was maintained at 25°C, the rotation speed was 200 r / min, and CO2-containing gas (purity>99%) was introduced into the reactor at a rate of 2 L / min, and the reaction was continued for 2 h.

[0078] (6) The mixed slurry after carbonization in (5) was placed in a container for 7 days. The mixed slurry after 7 days was mixed with 60 parts of ordinary Portland cement and added into a stirrer. The mixture was slowly stirred at a rate of 150 r / min for 1 min, and then quickly stirred at a rate of 400 r / min for 2 min to obtain a cement slurry. The mixture was poured into a mold and vibrated to form a dense shape. The mixture was demolded after 1 day. After standard curing for 28 days, the compressive strength of the test block obtained after curing was tested according to GB / T17671-1999 Cement mortar strength test method (ISO method).

[0079] Comparative Example 1

[0080] Weigh 100 parts of ordinary Portland cement and 45 parts of distilled water and add them into a stirrer. Stir slowly at 150 r / min for 1 min and then stir quickly at 400 r / min for 2 min to obtain cement slurry. Pour the slurry into a mold and vibrate to compact it. Demould the slurry after 1 day. After standard curing for 28 days, test the compressive strength of the test block obtained after curing according to GB / T 17671-1999 Test method for strength of cement mortar (ISO method).

[0081] Comparative Example 2

[0082] (1) The collected waste concrete test blocks were crushed with a jaw crusher and sieved. Then, the broken blocks with a particle size greater than 4.75 mm were ground again with a planetary ball mill at a speed of 300 r / min for 8 min with a ball-to-material ratio of 6:1. The product was sieved through a 325-mesh sieve to obtain recycled concrete powder with a particle size of 0.045 mm.

[0083] (2) Weigh 40 parts of recycled concrete powder and 60 parts of ordinary Portland cement, add the powder and 45 parts of distilled water into a stirrer, stir slowly at a speed of 150 r / min for 1 min, and then stir quickly at a speed of 400 r / min for 2 min to obtain cement slurry, pour it into a mold, vibrate and compact it into shape, demold it after 1 day, and after standard curing for 28 days, test the compressive strength of the test block obtained after curing according to GB / T 17671-1999 Cement mortar strength test method (ISO method).

[0084] Comparative Example 3

[0085] (1) The collected waste concrete test blocks were crushed with a jaw crusher and sieved. Then, the broken blocks with a particle size greater than 4.75 mm were ground again with a planetary ball mill at a speed of 300 r / min for 8 min with a ball-to-material ratio of 2:1. The product was sieved through a 325-mesh sieve to obtain recycled concrete powder with a particle size of 0.045 mm.

[0086] (2) 15% KH550 was added dropwise to an ethanol solution having a volume ratio of ethanol to water of 2:1 to prepare a KH550 ethanol solution. The regenerated micropowder was weighed and mixed with the KH550 ethanol solution at a mass ratio of 1:10, heated to 80 degrees Celsius, and continuously stirred with a magnetic force at a speed of 200 r / min for 8 minutes.

[0087] (3) Weigh 2 parts of Bacillus powder and 10 parts of distilled water to prepare a microbial solution at room temperature. After the solution is prepared, add 0.1 parts of sucrose and place it in a constant temperature shaker for shaking and incubation at a speed of 200 r / min and a temperature of 25°C for 20 h.

[0088] (4) At room temperature, 4 parts of gas-phase nano-silica, 4 parts of nano-titanium dioxide powder, 8 parts of vanillin polyoxyethylene ether (VAEO8) and 35 parts of distilled water were weighed and added into a beaker. The mixture was stirred magnetically for 20 minutes to prepare a nano-silica & nano-titanium dioxide suspension. 40 parts of modified recycled concrete powder were weighed and mixed with the nano-silica & nano-titanium dioxide suspension to form a mixed slurry. The mixed slurry was subjected to microwave treatment at a power of 600 W for 3 minutes. After an interval of 2 minutes, the mixed slurry was subjected to microwave treatment at the same power for 3 minutes.

[0089] (5) The microwave-treated mixed slurry and the microbial solution were added to the reactor, the water temperature was maintained at 25°C, the rotation speed was 200 r / min, and CO2-containing gas (purity>99%) was introduced into the reactor at a rate of 2 L / min, and the reaction was continued for 2 h.

[0090] (6) The mixed slurry after carbonization in (5) was mixed with 60 parts of ordinary Portland cement and added into a stirrer. The mixture was slowly stirred at a speed of 150 r / min for 1 min and then quickly stirred at a speed of 400 r / min for 2 min to obtain a cement slurry. The slurry was poured into a mold and vibrated to form a dense shape. The slurry was demolded after 1 day. After standard curing for 28 days, the compressive strength of the test block obtained after curing was tested according to GB / T 17671-1999 Cement mortar strength test method (ISO method).

[0091] Comparative Example 4

[0092] (1) The collected waste concrete test blocks were crushed with a jaw crusher and sieved. Then, the broken blocks with a particle size greater than 4.75 mm were ground again with a planetary ball mill at a speed of 300 r / min for 8 min with a ball-to-material ratio of 6:1. The product was sieved through a 325-mesh sieve to obtain recycled concrete powder with a particle size of 0.045 mm.

[0093] (2) Weigh 40 parts of modified recycled concrete powder and add them into a reactor together with 45 parts of distilled water. Ensure that the water temperature is 25°C, the rotation speed is 200r / min, and CO2-containing gas (purity>99%) is introduced into the reactor at a rate of 2L / min. The reaction is continued for 2h.

[0094] (3) The mixed slurry after carbonization in (2) is placed in a container and stored for 7 days. The mixed slurry after storage for 7 days is mixed with 60 parts of ordinary Portland cement. The above powder and 45 parts of distilled water are added into a stirrer and slowly stirred at a speed of 150 r / min for 1 min, and then quickly stirred at a speed of 400 r / min for 2 min to obtain a cement slurry. The slurry is poured into a mold and vibrated to form a dense shape. The slurry is demolded after 1 day. After standard curing for 28 days, the compressive strength of the test block obtained after curing is tested according to GB / T 17671-1999 Cement mortar strength test method (ISO method).

[0095] Comparative Example 5

[0096] The experimental steps and parameters are the same as those of Example 2, with the only difference being that this example uses only an equal amount of nano-silicon dioxide instead of nano-silicon dioxide and nano-titanium dioxide.

[0097] Comparative Example 6

[0098] The experimental steps and parameters are the same as those in Example 2, except that this example uses an equal amount of nano-titanium dioxide instead of nano-silicon dioxide and nano-titanium dioxide.

[0099] Comparative Example 7

[0100] The experimental steps and parameters are the same as those in Example 2, except that carbon dioxide was not introduced into the reactor in this example.

[0101] Comparative Example 8

[0102] The experimental steps and parameters are similar to those in Example 2, except that the surfactant vanillin polyoxyethylene ether (VAEO8) is not used in this example.

[0103] As can be seen from Table 1, compared with Examples 1-3, the results show that with the increase of the content of nanomaterials, the compressive strength of cement paste shows a trend of first increasing and then decreasing, indicating that the more nanomaterials, the better, but there is an optimal range; compared with Comparative Examples 2 and 7, Examples 1-3 show that carbonization significantly improves the mechanical properties of cement paste containing recycled concrete powder, indicating that the carbonization process strengthens the mechanical properties and volcanic ash activity of recycled concrete powder. This is because carbon dioxide penetrates into the recycled concrete powder during the carbonization process and reacts with calcium hydroxide, calcium silicate hydrate (CSH) and unhydrated cement clinker to generate calcium carbonate and silica gel, resulting in the densification of the recycled concrete powder; compared with Comparative Example 3, the results of Example 2 show that the ball-to-material ratio during ball milling has an effect on the activation effect of the recycled concrete powder. A certain influence; compared with comparative example 4, the results of Example 4 show that the use of nano-silicon dioxide & nano-titanium dioxide suspension for carbonization is significantly better than ordinary wet carbonization, and the stability of the mixed slurry after carbonization is better. The carbonized nano-silicon dioxide & nano-titanium dioxide suspension is added to the cement slurry, which also improves the compressive strength of the slurry; compared with comparative examples 5-6, the results of Example 2 show that the simultaneous use of nano-silicon dioxide and nano-titanium dioxide has an obvious synergistic effect; compared with comparative example 7, the results of Example 2 show that the surfactant has a significant effect on the dispersion of nanomaterials and affects the mechanical properties of the final slurry. Compared with comparative example 1, the results of Examples 1-3 show that the treated recycled concrete powder can effectively replace cement, and the strength is significantly improved after replacement, with the highest increase of 14%.

[0104] Table 1 Cement paste ratio and mechanical properties

[0105]

[0106] The above is only a preferred embodiment of the invention, which is only used to illustrate but not to limit the invention. Various changes, modifications and even equivalent substitutions may be made within the spirit and scope of the claims of the invention, but will still be protected by the invention.

Claims

1. A method for modifying recycled concrete powder based on process control, characterized in that: The raw materials include: recycled concrete powder, silane coupling agent KH550, nano silicon dioxide, nano titanium dioxide, surfactant, Bacillus KW, sucrose, deionized water, and gas containing carbon dioxide; The method comprises the following steps implemented in sequence: 1) Grinding waste concrete to a target particle size to obtain recycled concrete powder; 2) Adsorbing silane coupling agent KH550 on the surface of recycled concrete powder; 3) drying the micro powder and cooling; 4) preparing a suspension of nano-silicon dioxide and nano-titanium dioxide containing a surfactant, wherein the total mass of the nano-silicon dioxide and nano-titanium dioxide accounts for 1-3% of the mass of the recycled concrete micropowder; mixing the recycled concrete micropowder cooled in step 3) with the nano-silicon dioxide and nano-titanium dioxide suspension to prepare a mixed slurry; 5) Add 1-2 g / L sucrose to the prepared Bacillus solution for cultivation; the Bacillus powder accounts for 1%-3% of the mass of the recycled concrete powder; 6) Pour the mixed slurry and the Bacillus solution into a reactor, heat the reactor in a water bath at 20-25° C., stir during heating, and introduce a gas containing carbon dioxide into the reactor at a rate of 1-3 L / min during stirring to ensure that the pressure in the reactor is 0.2-0.3 MPa. The reaction process lasts for 1-3 hours.

2. The modification method according to claim 1, characterized in that: The particle size of the recycled concrete powder satisfies D90=45 μm, that is, among all particles of the recycled concrete powder, particles with a particle size greater than 45 μm account for 10%, and particles with a particle size less than 45 μm account for 90%.

3. The modification method according to claim 1, characterized in that: The silane coupling agent KH550 exists in the form of a solution, and is prepared by adding 10-15% of KH550 to an ethanol solution and fully hydrolyzing it; the content of the ethanol solution is ethanol:water=2:1-3:

1.

4. The modification method according to claim 1, characterized in that: The nano silicon dioxide and the nano titanium dioxide are simultaneously present in a nano silicon dioxide & nano titanium dioxide suspension, which is prepared by mixing hydrophilic gas phase nano silicon dioxide and nano titanium dioxide powder with deionized water and then ultrasonically dispersing for 10-30 minutes; the average particle size of the nano silicon dioxide & nano titanium dioxide in the suspension is in the range of 15-20nm.

5. The modification method according to claim 4, characterized in that: The nano-silicon dioxide & nano-titanium dioxide suspension needs to be added with a surfactant vanillin polyoxyethylene ether (VAEO8) of the same mass as the nano-material, and magnetically stirred at a speed of 100-200 r / min for 15-30 min to ensure uniform dispersion of the nano-silicon dioxide and nano-titanium dioxide in the suspension.

6. The modification method according to claim 1, characterized in that: The Bacillus KW is prepared by weighing the bacterial powder at a ratio of 1-3% to prepare a microbial solution. After the solution is prepared, 1-2g / L of sucrose is added thereto, and the solution is placed in a constant temperature shaker and shaken for 15-20h at a speed of 150-200r / min and a temperature of 25-30°C.

7. The modification method according to claim 1, characterized in that: The modified recycled concrete powder is included in the water-cement ratio as a solid as an auxiliary cementitious material, and the nano-silicon dioxide & nano-titanium dioxide suspension is included in the water-cement ratio as a liquid.

8. The modification method according to any one of claims 1 to 7, characterized in that: The steps include: Step S1: crushing the collected waste concrete test blocks with a jaw crusher, and then grinding the broken blocks with a particle size greater than 4.75 mm with a ball mill again, and sieving the products to obtain recycled concrete powder, with a controlled particle size of 0.02-0.045 mm; Step S2: adding 10-15% KH550 to an ethanol solution to fully hydrolyze it, wherein the ethanol solution is ethanol:water=2:1-3:1, to obtain a KH550 ethanol solution; then, adding the obtained recycled concrete powder to the above solution, heating it to 60-85°C, and magnetically stirring it at a speed of 100-200 r / min for 1-2 hours to allow KH550 to be adsorbed on the surface of the recycled powder; Step S3: placing the recycled concrete powder obtained in step S2 in a constant temperature oven at 100-120° C., drying until the mass is constant, then taking it out and cooling it to room temperature; Step S4: preparing a suspension of nano-silicon dioxide & nano-titanium dioxide containing a surfactant, wherein the total mass of the nano-silicon dioxide & nano-titanium dioxide accounts for 1-3% of the mass of the recycled concrete powder; mixing the recycled concrete powder cooled in step S3 with the nano-silicon dioxide & nano-titanium dioxide suspension to prepare a mixed slurry; Step S5: treating the mixed slurry at a power of 500-700 W for 1-3 min, and then treating it again at the same power for 1-3 min after an interval of 1-2 min to make it preliminarily evenly dispersed; Step S6: weighing the Bacillus powder according to the ratio of 1-3% of the mass of the recycled concrete powder to prepare a microbial solution, and after the solution is prepared, adding 1-2g / L of sucrose thereto, placing it in a constant temperature shaker, and shaking and culturing it at a speed of 150-200r / min and a temperature of 25-30°C for 15-20h; Step S7: Pour the mixed slurry after microwave-assisted dispersion in step S5 and the microbial solution into a reactor, heat the reactor in a water bath at 20-25°C, and magnetically stir the recycled concrete powder and nano-silicon dioxide & nano-titanium dioxide suspension in the reactor at a speed of 200-300r / min during the heating process, and introduce carbon dioxide-containing gas into the reactor at a rate of 1-3L / min during the stirring process to ensure that the pressure in the reactor is 0.2-0.3MPa, and continue carbonization for 1-3h.

9. The modified recycled concrete powder obtained according to any one of the modification methods of claims 1 to 8.

10. The use of the modified recycled concrete powder according to claim 9 in cement paste, characterized in that: The modified recycled concrete powder replaces cement at a replacement rate of 40%.

Citation Information

Cited By

  • Method for preparing low-carbon waste incineration fly ash (MSWIFA) cement-based material through carbonization of modified nano solution and application of low-carbon waste incineration fly ash (MSWIFA) cement-based material

    CN119977383A

  • A method for preparing low-carbon waste incineration fly ash (MSWIFA) cement-based materials by modified nano-solution carbonization and its application.

    CN119977383B