Curing agent and method for treating disintegration of granite weathered soil at bottom of foundation pit when meeting water
A curing agent using cement, quicklime, desulfurized gypsum, and slag powder effectively solidifies weathered granite soil mud, addressing inefficiency and cost issues in existing treatments by forming durable gels and recycling industrial waste.
Patent Information
- Application Number
- CN202411195106.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods for treating weathered granite soil that disintegrates when exposed to water are inefficient and costly, primarily relying on large amounts of cement, which is expensive and environmentally unsustainable.
A curing agent composed of cement, quicklime, desulfurized gypsum, slag powder, and a water reducing agent is used to solidify the mud formed by disintegrated granite soil, leveraging chemical reactions to form stable calcium silicate hydrate and calcium sulfoaluminate gels, enhancing bonding and durability while utilizing industrial waste materials.
The curing agent achieves high-efficiency and low-cost solidification of mud, providing stable and durable results within 2 days, with improved compressive strength and reduced environmental impact through the use of recycled materials.
Smart Images

Figure CN119059787A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of construction engineering, in particular to a curing agent and a method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water. Background Art
[0002] In construction projects, excavation of foundation pits is the basic link of construction projects, and its construction quality is directly related to the stability and safety of the overall structure. However, in the process of foundation pit excavation, various complex geological conditions are often encountered, one of which is granite weathered soil. Granite weathered soil has strong water sensitivity, and the content of powder particles in the soil sample is relatively high. Under the action of water, the repulsion between particles is enhanced, and the bonding performance between particles is weak. It is easy to lose its adhesion characteristics and form a granular structure, resulting in stress imbalance in the soil body, thus causing stress concentration, and eventually softening the soil body, losing its bonding effect in the structure and disintegrating and destroying; especially when minerals such as kaolinite in granite weathered soil meet water, they will quickly disintegrate and soften. With the further action of water, the soil particles gradually disperse to form a muddy substance. The disintegration of weathered soil will threaten the safety of foundation pit construction and facilities in the foundation pit. The loose soil produced by the disintegration may cause the excavation surface of the foundation pit to become unstable, affecting the construction progress and quality. At the same time, the mud, sand and stones produced by the disintegration may block the drainage system in the foundation pit, exacerbating the problem of water accumulation. If at the bottom of the foundation pit, this collapse phenomenon is more obvious. Due to the back and forth disturbance of the excavator, the weathered soil collapses into mud, and the mud depth may quickly reach 0.3-0.5m, or even deeper; these muds have certain fluidity, suspension and plasticity. Generally speaking, the specific gravity of the mud is usually between 1.1-1.6, the sand content is usually between 5-30%, the clay content is usually between 10-50%, and the water content is usually between 40-80%. The existence of these muds not only seriously affects the excavation progress of the foundation pit, but also may threaten the stability of the foundation pit.
[0003] Therefore, an effective solidification measure is urgently needed to solve the problem of mud formed after the weathered granite soil disintegrates when it encounters water. At present, the common treatment method is to directly use cement to solidify the mud, but the amount of cement used is large and the price is expensive, which is not economical. Therefore, how to achieve efficient and low-cost solidification of the mud formed after the weathered granite soil disintegrates when it encounters water has become a problem that needs to be solved urgently. Summary of the invention
[0004] The problem solved by the invention is: how to realize high-efficiency and low-cost solidification of mud formed after granite weathered soil disintegrates when encountering water.
[0005] To solve the above problems, the present invention provides a curing agent, which comprises, by weight, 40-70 parts of cement, 2-16 parts of quicklime, 10-30 parts of desulfurized gypsum, 5-30 parts of slag powder, and 0.05-0.8 parts of water reducing agent.
[0006] Optionally, the cement is PO42.5 cement.
[0007] Optionally, the water reducing agent is a polycarboxylic acid-based water reducing agent.
[0008] Optionally, the slag powder is S95 grade granulated blast furnace slag.
[0009] The present invention also provides a method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water, based on the above-mentioned curing agent, comprising:
[0010] Step S1, adding a curing agent to the mud in the foundation pit to obtain a mixture; the mud is mud formed after the granite weathered soil disintegrates when it encounters water;
[0011] Step S2, stirring the mixture and then performing a curing process.
[0012] Optionally, in step S1, the water content of the mud is 40-80%.
[0013] Optionally, in step S1, the specific gravity of the mud is 1.1-1.3.
[0014] Optionally, in step S1, the sand content of the mud is 10-25%.
[0015] Optionally, in step S1, the mass ratio of the curing agent to the mud is (0.08-0.20):1.
[0016] Optionally, in step S2, the curing treatment time is 1.5-2.5 days.
[0017] Compared with the prior art, the curing agent provided by the present invention is composed of cement, quicklime, desulfurized gypsum, slag powder and a water reducing agent, wherein the tricalcium silicate and the dicalcium silicate in the cement can react with the water in the sludge to generate calcium silicate hydrate (CSH) gel and calcium hydroxide, the calcium silicate hydrate gel has a gelling property, can bond the soil particles in the mud together to form a stable structure, and achieve the effect of mud solidification, in addition, the calcium silicate hydrate has excellent durability, can enhance the water resistance and durability of the solidified mud, so that the solidified mud can maintain stable performance for a long time; the quicklime reacts with water to further generate calcium hydroxide, and during the solidification process, the calcium hydroxide can further react with the silicate in the cement to generate more calcium silicate hydrate (CSH) gel, thereby further improving the effect of mud solidification. Slag powder will undergo secondary hydration reaction under alkaline conditions (such as when calcium hydroxide is present) to generate hydrated calcium silicate (CSH) and hydrated calcium aluminate (CAH) gel, which is beneficial to further improve the curing effect of the mud; desulfurized gypsum provides sulfate ions during the cement hydration reaction, thereby promoting calcium silicate to generate hydrated calcium sulfoaluminate gel, which is beneficial to further improve the curing effect of the mud. In addition, calcium hydroxide and other alkaline substances produced by cement during the hydration process can react with aluminate minerals in the mud under alkaline conditions to generate calcium sulfoaluminate; quicklime reacts with water to generate calcium hydroxide, increasing the alkalinity of the system, which helps the aluminate minerals in the clay to react to generate calcium sulfoaluminate; calcium sulfoaluminate is a substance with strong cementing ability, which is beneficial to improve the density and strength of the mud after curing. In addition, the curing agent provided by the present invention uses industrial solid wastes such as desulfurized gypsum and slag powder as raw materials, which solves the problem of industrial solid waste recycling and reduces environmental pollution. In addition, compared with cement as a curing agent, the curing agent provided by the present invention can achieve similar curing effects at a smaller dosage, which helps to reduce costs. It is found through experiments that by using the curing agent provided by the present invention, the mud formed after the granite weathered soil disintegrates when it encounters water can be solidified in about 2 days, and the compressive strength of the solidified mud is relatively high. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of a process for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water according to an embodiment of the present invention;
[0019] Figure 2 is a cross-sectional view of a stirring device in an embodiment of the present invention;
[0020] Figure 3 This is a schematic diagram of the structure of a stirring paddle in an embodiment of the present invention;
[0021] Figure 4 This is a picture of the foundation pit before the mud solidifies in Example 1;
[0022] Figure 5This is a picture of the foundation pit after the mud solidifies in Example 1.
[0023] Description of reference numerals:
[0024] 1. Vertical rod; 2. Horizontal beam; 3. Agitator paddle; 301. Connecting ring; 302. Agitator blade; 4. First bracket; 5. Second bracket; 6. Horizontal rotating shaft; 7. Connector. DETAILED DESCRIPTION
[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0026] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0027] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0028] The present embodiment provides a curing agent, whose components include, by weight: cement: 40-70 parts, quicklime: 2-16 parts, desulfurized gypsum: 10-30 parts, slag powder: 5-30 parts, and water reducing agent: 0.05-0.8 parts.
[0029] The curing agent provided by the embodiment of the present invention is composed of cement, quicklime, desulfurized gypsum, slag powder and a water reducing agent, wherein the tricalcium silicate and the dicalcium silicate in the cement can react with the water in the sludge to generate calcium silicate hydrate (CSH) gel and calcium hydroxide, and the calcium silicate hydrate gel has a gelling property, which can bond the soil particles in the mud together to form a stable structure, thereby achieving the effect of mud solidification. In addition, the calcium silicate hydrate has excellent durability, which can enhance the water resistance and durability of the solidified mud, so that the solidified mud can maintain stable performance for a long time; the quicklime reacts with water to further generate calcium hydroxide, and during the solidification process, the calcium hydroxide can further react with the silicate in the cement to generate more calcium silicate hydrate (CSH) gel, thereby further improving the effect of mud solidification. Slag powder will undergo secondary hydration reaction under alkaline conditions (such as when calcium hydroxide is present) to generate hydrated calcium silicate (CSH) and hydrated calcium aluminate (CAH) gel, which is conducive to further improving the curing effect of the mud; desulfurized gypsum provides sulfate ions during the cement hydration reaction, thereby promoting calcium silicate to generate hydrated calcium sulfoaluminate gel, which is conducive to further improving the curing effect of the mud. In addition, the calcium hydroxide and other alkaline substances produced by cement during the hydration process can react with the aluminate minerals in the mud under alkaline conditions to generate calcium sulfoaluminate; quicklime reacts with water to generate calcium hydroxide, increasing the alkalinity of the system, which helps the aluminate minerals in the clay to react to generate calcium sulfoaluminate; calcium sulfoaluminate is a substance with strong cementing ability, which is conducive to improving the density and strength of the mud after curing. In addition, the curing agent provided by the present invention uses industrial solid wastes such as desulfurized gypsum and slag powder as raw materials, solves the problem of industrial solid waste recycling, and reduces environmental pollution. In addition, compared with cement as a curing agent, the curing agent provided by the embodiment of the present invention can achieve similar curing effects at a smaller dosage, which helps to reduce costs. It is found through experiments that by using the curing agent provided by the present invention, the mud formed after the granite weathered soil disintegrates when it encounters water can be solidified in about 2 days, and the compressive strength of the solidified mud is relatively high.
[0030] In some embodiments of the present invention, the cement is PO42.5 cement.
[0031] In some embodiments of the present invention, the water reducer is a polycarboxylic acid-based water reducer.
[0032] In some embodiments of the present invention, the slag powder is S95 grade granulated blast furnace slag.
[0033] like Figure 1 As shown, the embodiment of the present invention also provides a method for treating the disintegration of weathered granite soil at the bottom of a foundation pit when exposed to water, based on the above-mentioned curing agent, comprising:
[0034] Step S1, adding a curing agent to the mud in the foundation pit to obtain a mixture; the mud is mud formed after the granite weathered soil disintegrates when it encounters water;
[0035] Step S2, stirring the mixture and then performing a curing process.
[0036] In order to improve the stirring effect, in some embodiments of the present invention, the stirring process is performed using a specific stirring device, such as Figure 2 and Figure 3 As shown, the stirring device includes a vertical rod 1, a crossbeam 2, a stirring paddle 3 and a driving device (not shown in the figure), the crossbeam 2 is arranged at the lower end of the vertical rod 1, the left end of the crossbeam 2 is provided with a first bracket 4, the right end of the crossbeam 2 is provided with a second bracket 5, a horizontal rotating shaft 6 is arranged between the first bracket 4 and the second bracket 5, a plurality of stirring paddles 3 are arranged on the horizontal rotating shaft, and the plurality of stirring paddles 3 are arranged at intervals along the axial direction of the horizontal rotating shaft 6, the stirring paddle 3 includes a connecting ring 301 and a plurality of stirring blades 302 spirally distributed along the connecting ring, the connecting ring 301 is fixed on the horizontal rotating shaft 6, and the driving device is used to drive the horizontal rotating shaft to rotate. When in use, the excavator bucket is unloaded, and then the stirring device is installed on the bucket wall of the excavator through a connecting piece 7 (such as a bolt). The use of the stirring device in conjunction with the excavator can improve the mixing effect of the curing agent and the mud in the foundation pit, which is conducive to improving the processing efficiency of the mud.
[0037] In some embodiments of the present invention, in step S1, the water content of the mud is 40-80%.
[0038] In some embodiments of the present invention, in step S1, the specific gravity of the mud is 1.1-1.3.
[0039] In some embodiments of the present invention, in step S1, the sand content of the mud is 10-25%.
[0040] In some embodiments of the present invention, in step S1, the mass ratio of the curing agent to the mud is (0.08-0.20):1.
[0041] In some embodiments of the present invention, in step S2, the curing treatment time is 1.5-2.5 days.
[0042] The present invention is further described below in conjunction with specific embodiments.
[0043] Example 1
[0044] A1. Add a curing agent to the mud in the foundation pit to obtain a mixture; the mud is formed by the disintegration of granite weathered soil in contact with water; wherein, by weight, the components of the curing agent include: 55 parts of cement, 9 parts of quicklime, 20 parts of desulfurized gypsum, 15.6 parts of slag powder, and 0.4 parts of water reducer; the cement is PO42.5 cement, the water reducer is a polycarboxylic acid water reducer, and the slag powder is S95 grade granulated blast furnace slag; the mud is formed by the disintegration of granite weathered soil in contact with water, the water content of the mud is 60%, the specific gravity of the mud is 1.2, the sand content of the mud is 20%, and the mass ratio of the curing agent to the mud is 0.1:1.
[0045] A2. After stirring the mixture, curing is performed to obtain solidified mud; wherein the curing time is 2 days. Figure 4 This is a picture of the foundation pit before the mud solidifies. Figure 5 This is a picture of the foundation pit after the mud solidifies. Figure 4 and Figure 5 It can be seen that the solidification effect of the mud in the foundation pit in Example 1 is good.
[0046] Example 2
[0047] The difference from Example 1 is that, by weight, the components of the curing agent include: cement: 40 parts, quicklime: 16 parts, desulfurized gypsum: 22 parts, slag powder: 21.2 parts, and water reducing agent: 0.8 parts.
[0048] Example 3
[0049] The difference from Example 1 is that, by weight, the components of the curing agent include: cement: 70 parts, quicklime: 12 parts, desulfurized gypsum: 10 parts, slag powder: 7.9 parts, and water reducing agent: 0.1 parts.
[0050] Experimental example
[0051] The compressive strength of the solidified muds prepared in Examples 1-3 was tested, and the results are shown in Table 1. As can be seen from Table 1, the compressive strength of the solidified muds in Examples 1-3 is relatively high, which are 1.41 MPa, 1.42 MPa and 1.45 MPa, respectively.
[0052] Table 1
[0053]
[0054] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A curing agent, characterized in that Calculated by weight, the components include: cement: 40-70 parts, quicklime: 2-16 parts, desulfurized gypsum: 10-30 parts, slag powder: 5-30 parts, and water reducing agent: 0.05-0.8 parts.
2. The curing agent according to claim 1, characterized in that The cement is PO42.5 cement.
3. The curing agent according to claim 1, characterized in that The water reducing agent is a polycarboxylic acid water reducing agent.
4. The curing agent according to claim 1, characterized in that The slag powder is S95 grade granulated blast furnace slag.
5. A method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water, based on the curing agent according to any one of claims 1 to 4, characterized in that: include: Step S1, adding a curing agent to the mud in the foundation pit to obtain a mixture; the mud is mud formed after the granite weathered soil disintegrates when it encounters water; Step S2, stirring the mixture and then performing a curing process.
6. The method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water according to claim 5, characterized in that: In the step S1, the water content of the mud is 40-80%.
7. The method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water according to claim 5, characterized in that: In the step S1, the specific gravity of the mud is 1.1-1.
3.
8. The method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water according to claim 5, characterized in that: In the step S1, the sand content of the mud is 10-25%.
9. The method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water according to claim 5, characterized in that: In the step S1, the mass ratio of the curing agent to the mud is (0.08-0.20):
1.
10. The method for treating weathered granite soil at the bottom of a foundation pit that disintegrates when exposed to water according to claim 5, characterized in that: In step S2, the curing treatment time is 1.5-2.5 days.
Citation Information
Cited By
Modifier for dewatering modification treatment of engineering waste slurry and use method of modifier
CN121225852A