Lead-free piezoelectric ceramic with high Curie temperature and preparation method thereof
By introducing SiO2 into lead-free piezoelectric ceramics to form the second phase, using its enrichment characteristics at the grain boundary, the problem that Curie temperature and piezoelectric constant are difficult to increase simultaneously in the traditional method, and the piezoelectric constant is achieved while maintaining the piezoelectric constant. The effect of significantly increasing Curie temperature while decreasing.
Patent Information
- Application Number
- CN202410966039.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-18
AI Technical Summary
While the existing lead-free piezoelectric ceramics are difficult to keep the piezoelectric constant from falling while increasing the Curie temperature, and traditional chemical doping methods cannot increase the Curie temperature and piezoelectric constant at the same time.
Ba(Hf0.02Ti0.98)O3-xSiO2 is used as the lead-free piezoelectric ceramic matrix, and the second phase is formed by introducing SiO2, and a new chemical modification method is adopted to enrich SiO2 at the grain boundary to hinder the ferroelectric phase transformation and improve the Curie temperature.
While ensuring that the piezoelectric constant does not decrease, the Curie temperature of lead-free piezoelectric ceramics is significantly increased. Through the formation and distribution of the second phase of SiO2, the ferroelectric phase transformation is effectively hindered and the use temperature range of the ceramics is increased.
Smart Images

Figure CN119059810A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piezoelectric ceramics, and in particular to a lead-free piezoelectric ceramic with a high Curie temperature and a preparation method thereof. Background Art
[0002] In the information age, the discovery and application of piezoelectric materials have provided new solutions for information transmission and energy conversion, fully demonstrating the key role of materials science in the advancement of modern technology. Among them, piezoelectric ceramics, as an important functional material for realizing the mutual conversion of mechanical energy and electrical energy, play an irreplaceable role in key fields such as aerospace, medical equipment, precision measurement, and electronic information technology due to their unique physical properties.
[0003] In the classification of piezoelectric materials, according to the different constituent elements, they are mainly divided into two categories: lead-based and lead-free piezoelectric ceramics. Lead-based piezoelectric ceramics Pb(Zr, Ti)O3(PZT) are currently the most widely used piezoelectric materials. However, the widespread use of lead-based piezoelectric ceramics has brought concerns about environmental pollution and human health. During the high-temperature production process, the volatilization of lead may pollute the environment. At the same time, long-term exposure to an environment with excessive lead content may cause health risks including nervous system damage, cardiovascular disease, osteoporosis, reproductive system disorders and decreased immune function, and these effects are often irreversible. With people's increasing concern about environmental pollution and physical health, the world has begun to formulate and implement a series of laws and regulations aimed at restricting the use of lead-containing materials. Under such an international background, the development of lead-free piezoelectric ceramics to replace traditional lead-based piezoelectric materials is not only a need to respond to regulatory restrictions, but also conforms to the scientific trend of sustainable development and environmental protection requirements. my country is the world's largest industrial country and the largest exporter of industrial products. With the implementation of relevant national laws, exports to relevant countries will inevitably be restricted. In order to avoid unrestricted related products, it is urgent to develop products that can replace lead-based piezoelectric ceramics.
[0004] Chemical doping is the most common piezoelectric ceramic modification technology. It changes the microstructure of the raw materials by doping ions of different radii, thereby adjusting the performance of piezoelectric ceramics. Conventional doping methods include isovalent doping and heterovalent doping, both of which will bring microstructure changes to piezoelectric ceramics, resulting in changes in performance. Changes in microstructure directly affect various properties of piezoelectric ceramics, such as Curie temperature, piezoelectric constant, etc.
[0005] The Curie temperature marks the critical point where ferroelectric or ferroelectric materials transform into paraelectric materials. In other words, the Curie temperature directly affects the temperature range of piezoelectric ceramics, and is one of the important performance parameters of BT-based piezoelectric ceramics. The proportional constant that describes the linear response relationship between the mechanical and electrical quantities of a piezoelectric body is called the piezoelectric constant, which is also an important performance parameter of BT-based piezoelectric ceramics. However, in traditional chemical doping, the Curie temperature and the piezoelectric constant cannot be improved at the same time, nor can it be guaranteed that one of the performance parameters will be effectively improved without decreasing the other performance parameter. Summary of the invention
[0006] In order to achieve the above object, the present invention aims to provide a lead-free piezoelectric ceramic with a high Curie temperature and a preparation method thereof, which can increase the Curie temperature of the lead-free piezoelectric ceramic while ensuring that the piezoelectric constant does not decrease.
[0007] In order to achieve the above object, the present invention provides a lead-free piezoelectric ceramic with a high Curie temperature. The expression of the lead-free piezoelectric ceramic is Ba(Hf 0.02 Ti 0.98 )O3-xSiO2, where x=0~1.5.
[0008] The present invention also provides a method for preparing a lead-free piezoelectric ceramic with a high Curie temperature, comprising the following steps:
[0009] S1: Weigh BaCO3, TiO2, HfO2, and SiO2 powders in proportion;
[0010] S2: ball milling the weighed powder for the first time, followed by drying and sieving;
[0011] S3: pre-calcining the powder, and then ball-milling the powder for the second time, drying and sieving the ball-milled powder;
[0012] S4: adding paraffin wax to the sieved powder to granulate, and forming a ceramic body from the granulated ceramic powder;
[0013] S5: placing the ceramic body into a tube furnace for debinding and sintering to obtain lead-free piezoelectric ceramics.
[0014] In the above scheme: the particle size of BaCO3, TiO2, HfO2, and SiO2 powders is 0.1-5 μm, and the purity is greater than 99.0%.
[0015] In the above scheme: in step S2, anhydrous ethanol is first added to the weighed powder, and then the first ball milling is performed to prevent the powder from sticking.
[0016] In the above scheme: the ratio of weighed powder and anhydrous ethanol is 1g:1.5-2ml.
[0017] In the above scheme: the ball milling parameters for the first ball milling and the second ball milling are: ball milling speed 300-400rpm / min, ball milling time 12-24h, the ball milling beads used for ball milling are ZrO2 with a purity of 95%, and the ball mill includes three types of ball milling beads with diameters of 1mm, 3mm, and 5mm, respectively, and the corresponding mass ratio is 1:3:5.
[0018] In the above scheme: in step S4, the mass of the added paraffin is 6%-8% of the mass of the powder.
[0019] In the above scheme: in step S5, the debinding temperature is 600-650°C, and the temperature is kept for 4 hours; the solid phase sintering method is adopted, and the sintering temperature is 1300-1400°C, wherein the heating rate from room temperature to 600°C is 5°C / min; the heating rate from 600°C to 1100°C is 4°C / min; the heating rate from 1100°C to 1400°C is 3°C / min.
[0020] The beneficial effects of the present invention are: the use of Ba(Hf 0.02 Ti 0.98 )O3(BHT) is used as the matrix, and a new type of chemical modification method is adopted, which is different from the common isovalent and alivalent doping, to introduce SiO2 to add the second phase to increase the Curie temperature; in the process of SiO2 entering the BHT ceramic matrix, the formed second phase is enriched at the grain boundary in the form of independent grains. When the temperature rises to near the Curie temperature, the second phase enriched at the grain boundary will hinder the transformation of the ferroelectric phase into the paraelectric phase, thereby achieving the purpose of increasing the Curie temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0022] Figure 1 XRD patterns of lead-free piezoelectric ceramics. (a) XRD pattern. (b) Locally enlarged XRD pattern.
[0023] Figure 2 SEM and EDS images of lead-free piezoelectric ceramics. (a)-(d) SEM morphology and grain size distribution of ceramics; (e) Relationship curve between grain size and SiO2 content; (f) Enlarged image of morphology area.
[0024] Figure 3 The dielectric temperature spectrum test diagram of lead-free piezoelectric ceramics. (a)-(d)ε r -T and tanδ-T curves; (e) Schematic diagram of grain equivalent capacitor.
[0025] Figure 4 This is a test chart of the ferroelectric and piezoelectric properties of lead-free piezoelectric ceramics. DETAILED DESCRIPTION
[0026] like Figure 1 As shown in FIG. 4 , a lead-free piezoelectric ceramic with a high Curie temperature is expressed as Ba(Hf 0.02 Ti 0.98 )O3-xSiO2, where x = 0 to 1.5. The specific chemical composition is shown in Table 1.
[0027] Table 1Ba(Hf 0.02 Ti 0.98 )O3-xSiO2 lead-free piezoelectric ceramic chemical composition
[0028]
[0029] The present invention also proposes a method for preparing a lead-free piezoelectric ceramic with a high Curie temperature, which mainly comprises the following steps:
[0030] S1: Weigh BaCO3, TiO2, HfO2, and SiO2 powders in proportion, with a powder particle size of 0.1 to 5 μm and a purity greater than 99.0%.
[0031] S2: The weighed powder is ball-milled for the first time. Anhydrous ethanol is added before ball-milling to prevent the powder from sticking. The ratio of the weighed powder to anhydrous ethanol is 1g:1.5-2ml. After ball-milling, the powder is dried and sieved.
[0032] S3: pre-sintering the powder, and then ball-milling the powder for the second time, drying and sieving the ball-milled powder.
[0033] The ball milling parameters for the first and second ball milling are: ball milling speed 300-400rpm / min, ball milling time 12-24h, the ball milling beads used for ball milling are ZrO2 with a purity of 95%, and the ball mill includes three diameters of ball milling beads, namely 1mm, 3mm, and 5mm, and the corresponding mass ratio is 1:3:5.
[0034] S4: adding paraffin wax to the sieved powder for granulation, wherein the mass of the added paraffin wax is 6%-8% of the mass of the powder, and the granulated ceramic powder is made into a ceramic body.
[0035] S5: placing the ceramic body into a tubular furnace for debinding and sintering to obtain lead-free piezoelectric ceramics; the debinding temperature is 600-650°C, and the temperature is kept for 4 hours; a solid phase sintering method is adopted, and the sintering temperature is 1300-1400°C, wherein the heating rate from room temperature to 600°C is 5°C / min; the heating rate from 600°C to 1100°C is 4°C / min; the heating rate from 1100°C to 1400°C is 3°C / min.
[0036] Example 1
[0037] S1: According to Ba(Hf 0.02 Ti 0.98 )O3-xSiO2, x=0 Weigh BaCO3, TiO2, HfO2, and SiO2 powders, each with a particle size of 0.1 to 5 μm and a purity greater than 99.0%.
[0038] S2: Transfer the weighed powder to a nylon ball mill for the first ball milling. Add anhydrous ethanol before ball milling to prevent the powder from sticking. The ratio of weighed powder to anhydrous ethanol is 90 ml of anhydrous ethanol for every 50 g of ceramic powder. Ball milling parameters are: ball milling speed 300 rpm / min, ball milling time 12 h, ball milling beads used for ball milling are 95% pure ZrO2, and the ball mill includes three diameters of ball milling beads, namely 1 mm, 3 mm, and 5 mm, and the corresponding mass ratio is 1:3:5. Transfer the ball milled powder to an oven and dry it at 60 ° C for 10 h; after drying, separate the ceramic powder and ball milling beads with a standard sieve of 80 mesh.
[0039] S3: The powder is placed in a corundum crucible for pre-sintering at a temperature of 1200°C for 3 hours. After the pre-sintering, the powder is ball-milled for the second time, and the ball-milled powder is dried and sieved. The details are the same as the first ball milling.
[0040] S4: paraffin wax is added to the sieved powder for granulation, the mass of the added paraffin wax is 6% of the mass of the powder, and the granulated ceramic powder is pressed at 30 MPa to form a disc-shaped ceramic body with a diameter of 1.2 mm and a diameter of 1.1 mm.
[0041] S5: Place the ceramic body into a tubular furnace for debinding and sintering to obtain lead-free piezoelectric ceramics; the debinding temperature is 600°C and kept warm for 4 hours; a solid phase sintering method is adopted with a sintering temperature of 1300-1400°C, wherein the heating rate from room temperature to 600°C is 5°C / min; the heating rate from 600°C to 1100°C is 4°C / min; the heating rate from 1100°C to 1400°C is 3°C / min, thus obtaining the final ceramic sample.
[0042] S6: Finally, silver paste is applied to both electrodes of the ceramic sample and silver is fired according to the test requirements.
[0043] Example 2
[0044] S1: According to Ba(Hf 0.02 Ti 0.98 )O3-xSiO2, x=0.5 Weigh BaCO3, TiO2, HfO2, and SiO2 powders, each with a particle size of 0.1 to 5 μm and a purity greater than 99.0%.
[0045] S2: Transfer the weighed powder to a nylon ball mill for the first ball milling. Add anhydrous ethanol before ball milling to prevent the powder from sticking. The ratio of weighed powder to anhydrous ethanol is 90 ml of anhydrous ethanol for every 50 g of ceramic powder. Ball milling parameters are: ball milling speed 300 rpm / min, ball milling time 12 h, ball milling beads used for ball milling are 95% pure ZrO2, and the ball mill includes three diameters of ball milling beads, namely 1 mm, 3 mm, and 5 mm, and the corresponding mass ratio is 1:3:5. Transfer the ball milled powder to an oven and dry it at 60 ° C for 10 h; after drying, separate the ceramic powder and ball milling beads with a standard sieve of 80 mesh.
[0046] S3: The powder is placed in a corundum crucible for pre-sintering at a temperature of 1200°C for 3 hours. After the pre-sintering, the powder is ball-milled for the second time, and the ball-milled powder is dried and sieved. The details are the same as the first ball milling.
[0047] S4: paraffin wax is added to the sieved powder for granulation, the mass of the added paraffin wax is 6% of the mass of the powder, and the granulated ceramic powder is pressed at 30 MPa to form a disc-shaped ceramic body with a diameter of 1.2 mm and a diameter of 1.1 mm.
[0048] S5: Place the ceramic body into a tubular furnace for debinding and sintering to obtain lead-free piezoelectric ceramics; the debinding temperature is 600°C and kept warm for 4 hours; a solid phase sintering method is adopted with a sintering temperature of 1300-1400°C, wherein the heating rate from room temperature to 600°C is 5°C / min; the heating rate from 600°C to 1100°C is 4°C / min; the heating rate from 1100°C to 1400°C is 3°C / min, thus obtaining the final ceramic sample.
[0049] S6: Finally, silver paste is applied to both electrodes of the ceramic sample and silver is fired according to the test requirements.
[0050] Example 3
[0051] S1: According to Ba(Hf 0.02 Ti 0.98 )O3-xSiO2, x=1.0 Weigh BaCO3, TiO2, HfO2, and SiO2 powders, each with a particle size of 0.1 to 5 μm and a purity greater than 99.0%.
[0052] S2: Transfer the weighed powder to a nylon ball mill for the first ball milling. Add anhydrous ethanol before ball milling to prevent the powder from sticking. The ratio of weighed powder to anhydrous ethanol is 90 ml of anhydrous ethanol for every 50 g of ceramic powder. Ball milling parameters are: ball milling speed 300 rpm / min, ball milling time 12 h, ball milling beads used for ball milling are 95% pure ZrO2, and the ball mill includes three diameters of ball milling beads, namely 1 mm, 3 mm, and 5 mm, and the corresponding mass ratio is 1:3:5. Transfer the ball milled powder to an oven and dry it at 60 ° C for 10 h; after drying, separate the ceramic powder and ball milling beads with a standard sieve of 80 mesh.
[0053] S3: The powder is placed in a corundum crucible for pre-sintering at a temperature of 1200°C for 3 hours. After the pre-sintering, the powder is ball-milled for the second time, and the ball-milled powder is dried and sieved. The details are the same as the first ball milling.
[0054] S4: paraffin wax is added to the sieved powder for granulation, the mass of the added paraffin wax is 6% of the mass of the powder, and the granulated ceramic powder is pressed at 30 MPa to form a disc-shaped ceramic body with a diameter of 1.2 mm and a diameter of 1.1 mm.
[0055] S5: Place the ceramic body into a tubular furnace for debinding and sintering to obtain lead-free piezoelectric ceramics; the debinding temperature is 600°C and kept warm for 4 hours; a solid phase sintering method is adopted with a sintering temperature of 1300-1400°C, wherein the heating rate from room temperature to 600°C is 5°C / min; the heating rate from 600°C to 1100°C is 4°C / min; the heating rate from 1100°C to 1400°C is 3°C / min, thus obtaining the final ceramic sample.
[0056] S6: Finally, silver paste is applied to both electrodes of the ceramic sample and silver is fired according to the test requirements.
[0057] Example 4
[0058] S1: According to Ba(Hf 0.02 Ti 0.98 )O3-xSiO2, x=1.5 Weigh BaCO3, TiO2, HfO2, and SiO2 powders, each with a particle size of 0.1 to 5 μm and a purity greater than 99.0%.
[0059] S2: Transfer the weighed powder to a nylon ball mill for the first ball milling. Add anhydrous ethanol before ball milling to prevent the powder from sticking. The ratio of weighed powder to anhydrous ethanol is 90 ml of anhydrous ethanol for every 50 g of ceramic powder. Ball milling parameters are: ball milling speed 300 rpm / min, ball milling time 12 h, ball milling beads used for ball milling are 95% pure ZrO2, and the ball mill includes three diameters of ball milling beads, namely 1 mm, 3 mm, and 5 mm, and the corresponding mass ratio is 1:3:5. Transfer the ball milled powder to an oven and dry it at 60 ° C for 10 h; after drying, separate the ceramic powder and ball milling beads with a standard sieve of 80 mesh.
[0060] S3: The powder is placed in a corundum crucible for pre-sintering at a temperature of 1200°C for 3 hours. After the pre-sintering, the powder is ball-milled for the second time, and the ball-milled powder is dried and sieved. The details are the same as the first ball milling.
[0061] S4: paraffin wax is added to the sieved powder for granulation, the mass of the added paraffin wax is 6% of the mass of the powder, and the granulated ceramic powder is pressed at 30 MPa to form a disc-shaped ceramic body with a diameter of 1.2 mm and a diameter of 1.1 mm.
[0062] S5: Place the ceramic body into a tubular furnace for debinding and sintering to obtain lead-free piezoelectric ceramics; the debinding temperature is 600°C and kept warm for 4 hours; a solid phase sintering method is adopted with a sintering temperature of 1300-1400°C, wherein the heating rate from room temperature to 600°C is 5°C / min; the heating rate from 600°C to 1100°C is 4°C / min; the heating rate from 1100°C to 1400°C is 3°C / min, thus obtaining the final ceramic sample.
[0063] S6: Finally, silver paste is applied to both electrodes of the ceramic sample and silver is fired according to the test requirements.
[0064] Figure 1 XRD spectrum of lead-free piezoelectric ceramics. (a) XRD spectrum. (b) Locally enlarged XRD spectrum. The second phase was detected in all samples with x=0.5-1.5w%. By comparing with the standard card, it is known that the second phase is Ba2TiSi2O8 and Ba2SiO8, both of which are oxides containing Si; by comparing the diffraction peaks of the standard card, it can be seen that the 45° characteristic peak of x=0w% is split into obvious T(002) and O(022), O(200) diffraction peaks, indicating that it is the coexistence of OT two phases at room temperature.
[0065] Figure 2 SEM and EDS of lead-free piezoelectric ceramics; (a)-(d) SEM morphology and grain size distribution of ceramics; (e) Relationship curve between grain size and SiO2 content; (f) Enlarged view of morphology area; Figure 2It is observed in (a)-(e) that when x=0w%, the grain size is larger (=30.33μm), and when SiO2 is added, it immediately decreases to 0.6μm. As the SiO2 content increases, the grain size increases again. This is because during sintering, the increase of the second phase brings about the increase of the liquid phase, which slightly increases its grain size. The influence of the liquid phase and the influence of the second phase as a grain growth inhibitor exist simultaneously. Figure 2 EDS element analysis of the three points in (f) shows that the second phase rich in Si is embedded in the BHT ceramic grains.
[0066] Figure 3 Dielectric temperature spectrum test of lead-free piezoelectric ceramics. (a)-(d)ε r -T and tanδ-T curves; (e) Schematic diagram of grain equivalent capacitor; Figure 3 From (a)-(d), we can see that at T C Nearby ε r The -T curve shows that it gradually changes from sharp and narrow to round and blunt divergence with the increase of the second phase, which indicates that the diffuse phase transition behavior of the sample increases with the increase of the second phase; Figure 3 (d) It can be observed that T C Compared with (a), it is increased by 14 degrees, proving that this method can increase the Curie temperature; as shown in Figure 3(e), when the electric field E is fixed, ε r It decreases with the increase of grain size.
[0067] Figure 4 It is the test of ferroelectric and piezoelectric properties of lead-free piezoelectric ceramics, specifically the content of the second phase (Ba2TiSi2O8), Curie temperature T C and the piezoelectric constant d 33 As x changes, the curve Figure 4 As shown, it can be found that d 33 First, it decreases rapidly from x = 0w% to x = 0.5w%, and then d 33 The decrease in T is very slight and can be almost ignored. C The trend of change is just the opposite, rising slowly from x = 0w% to x = 0.5w%, and then T C Rapidly rise to 134.7℃.
Claims
1. A lead-free piezoelectric ceramic with a high Curie temperature, characterized in that: The expression of the lead-free piezoelectric ceramic is Ba(Hf 0.02 Ti 0.98 )O3-xSiO2, where x=0~1.
5.
2. A method for preparing a lead-free piezoelectric ceramic with a high Curie temperature according to claim 1, characterized in that: The following steps are involved: S1: Weigh BaCO3, TiO2, HfO2, and SiO2 powders in proportion; S2: ball milling the weighed powder for the first time, followed by drying and sieving; S3: pre-calcining the powder, and then ball-milling the powder for the second time, drying and sieving the ball-milled powder; S4: adding paraffin wax to the sieved powder to granulate, and forming a ceramic body from the granulated ceramic powder; S5: placing the ceramic body into a tube furnace for debinding and sintering to obtain lead-free piezoelectric ceramics.
3. The method for preparing a lead-free piezoelectric ceramic with a high Curie temperature according to claim 2, characterized in that: The particle size of BaCO3, TiO2, HfO2 and SiO2 powders is 0.1-5 μm, and the purity is greater than 99.0%.
4. The method for preparing a lead-free piezoelectric ceramic with a high Curie temperature according to claim 2, characterized in that: In step S2, anhydrous ethanol is first added to the weighed powder, and then the first ball milling is performed.
5. The method for preparing a lead-free piezoelectric ceramic with a high Curie temperature according to claim 4, characterized in that: The weighed powder and anhydrous ethanol are mixed in a ratio of 1g:1.5-2ml.
6. The method for preparing a lead-free piezoelectric ceramic with a high Curie temperature according to claim 4, characterized in that: The ball milling parameters for the first and second ball milling are: ball milling speed 300-400rpm / min, ball milling time 12-24h, the ball milling beads used for ball milling are ZrO2 with a purity of 95%, and the ball mill includes three diameters of ball milling beads, namely 1mm, 3mm, and 5mm, and the corresponding mass ratio is 1:3:
5.
7. The method for preparing a lead-free piezoelectric ceramic with a high Curie temperature according to claim 2, characterized in that: In step S4, the mass of the added paraffin is 6%-8% of the mass of the powder.
8. The method for preparing a lead-free piezoelectric ceramic with a high Curie temperature according to claim 2, characterized in that: In step S5, the debinding temperature is 600-650°C and kept warm for 4 hours; the solid phase sintering method is adopted, and the sintering temperature is 1300-1400°C, wherein the heating rate from room temperature to 600°C is 5°C / min; the heating rate from 600°C to 1100°C is 4°C / min; the heating rate from 1100°C to 1400°C is 3°C / min.
Citation Information
Patent Citations
High-dielectric constant ceramic composite and ceramic capacitor elements
CA2006664A1
Barium hafnium titanate leadless piezoelectric ceramic with high piezoelectric coefficient and preparation method of leadless piezoelectric ceramic
CN103467085A
Barium titanate-based leadless piezoelectric ceramic and preparation method thereof
CN104016674A
Bismuth ferrite-barium titanate lead-free piezoelectric ceramic material and preparation method thereof
CN115101659A
High-strain bismuth ferrite-based leadless piezoelectric ceramic and preparation method thereof
CN118084471A