Cycloolefin monomer, cycloolefin ring-opening polymer prepared from cycloolefin monomer as well as preparation method and application of cycloolefin ring-opening polymer

By using norbornene derivatives with fused ring aromatic hydrocarbon substituents as cycloolefin monomers, the problems of low glass transition temperature and poor heat resistance of existing cycloolefin copolymers were solved, and a high-performance cycloolefin ring-opening polymer was prepared. , suitable for the manufacturing of high-end optical components.

CN119059872APending Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310645712.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The cycloolefin copolymers produced by existing cycloolefin monomers have low glass transition temperature and poor heat resistance, making it difficult to meet the needs of high-end electronic devices or display devices.

Method used

Using norbornene derivatives containing fused ring aromatic hydrocarbon substituents as cycloolefin monomers, react with dienols and dienols under the protection of inert gas to obtain cycloolefin monomers with high steric hindrance and rigidity, and in the catalyst The ring-opening metathesis polymerization reaction was carried out in presence and then hydroreduction was carried out to prepare a cycloolefin ring-opening polymer with high glass transition temperature, heat resistance and refractive index.

Benefits of technology

It realizes the high glass transition temperature, high heat resistance and high refractive index of cycloolefin ring-opening polymer, and is suitable for the preparation of optical components such as smartphones, microscope optical lenses and light guide plates for liquid crystal screens.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059872A_ABST
    Figure CN119059872A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of optical materials, and discloses a cycloolefin monomer, a cycloolefin ring-opening polymer prepared from the cycloolefin monomer, and a preparation method and application of the cycloolefin ring-opening polymer. The structure of the cycloolefin monomer is as shown in formula I: in the formula I, L is 0, 1 or 2; ar represents an aromatic hydrocarbon substituent group or an aza-aryl group. The cycloolefin monomer provided by the invention is a norbornene derivative containing a polycyclic aromatic hydrocarbon substituent group, and compared with norbornene without a substituent group or substituted by an alkyl group, after the polycyclic aromatic hydrocarbon substituent group is introduced, the monomer has higher steric hindrance and rigidity, and a homopolymer shows higher glass transition temperature and better heat resistance. The method is suitable for preparing molding materials of optical elements such as optical lenses of smart phones and microscopes and light guide plates of liquid crystal screens. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical materials, and in particular to a cycloolefin monomer and a cycloolefin ring-opening polymer prepared therefrom, and a preparation method and application thereof. Background Art

[0002] Cyclo Olefin Polymer (COP) is a non-crystalline homopolymer formed by the ring-opening heteropolymerization of bicycloheptene (norbornene) under the action of metallocene catalysts and then hydrogenation reaction. Because cycloolefin polymers have excellent optical properties such as good processing performance, high light transmittance, low birefringence, low hygroscopicity, and light weight, they are widely used as key molding materials for optical components such as optical lenses and light guide plates. In recent years, it has replaced high-end materials such as glass and other plastic packaging and has been widely used in medical, pharmaceutical and cosmetic fields such as prefilled syringes, plastic vials, infusion bags, contrast agents, hyaluronic acid packaging bottles, etc.

[0003] As electronic products continue to develop towards ultra-thinness and high integration, the requirements for optical resin materials in terms of lightness, heat resistance, and high-temperature dimensional stability are becoming increasingly higher. Although cycloolefin polymer materials have excellent optical properties, polymers prepared using conventional norbornene monomers still have certain defects.

[0004] JP2008-144013 discloses a method for preparing an addition copolymer of norbornene monomer and ethylene. The refractive index and glass transition temperature of the copolymer are higher than those of optical materials such as PC and PMMA, and can effectively reduce aberration and distortion in optical systems; however, the refractive index, glass transition temperature and heat resistance of the copolymer are lower than those of cyclic olefin copolymer materials, and it is difficult to meet the requirements of some high-end electronic devices or display devices.

[0005] CN109134755A discloses a heat-resistant cycloolefin copolymer and a preparation method thereof, specifically a copolymer of a norbornene derivative 5-ethylidene-2-norbornene and a long-chain alpha olefin such as 1-hexene- and 1-octene-. The preparation method of the invention has the advantages of mild reaction conditions, short cycle, simple operation, etc., and has great industrial application value and good application prospects. However, the heat resistance of the cycloolefin copolymer obtained by using such monomers is insufficient, and it is difficult to meet the needs of some high-end electronic devices or display devices. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of low glass transition temperature and poor heat resistance of cycloolefin copolymers prepared from cycloolefin monomers in the prior art, and to provide cycloolefin monomers and cycloolefin ring-opening polymers prepared therefrom, as well as preparation methods and applications thereof. The cycloolefin ring-opening polymers prepared from the cycloolefin monomers of the present invention have the advantages of high glass transition temperature, high heat resistance, high refractive index and easy processing.

[0007] In order to achieve the above object, the first aspect of the present invention provides a cycloolefin monomer, the structure of which is shown in Formula I:

[0008]

[0009] In Formula I,

[0010] L is 0, 1 or 2;

[0011] Ar represents an aromatic hydrocarbon substituent or an azaaryl group.

[0012] A second aspect of the present invention provides a method for preparing a cycloolefin monomer, the preparation method comprising:

[0013] Under the protection of an inert gas, a diene and a dienophile are reacted in a solvent to obtain the cycloolefin monomer; wherein the structure of the cycloolefin monomer is as shown in Formula I:

[0014]

[0015] In Formula I,

[0016] L is 0, 1 or 2;

[0017] Ar represents an aromatic hydrocarbon substituent or an azaaryl group.

[0018] The third aspect of the present invention provides a cycloolefin monomer prepared by the preparation method of the second aspect.

[0019] A fourth aspect of the present invention provides use of the aforementioned cycloolefin monomer in the preparation of an optical resin.

[0020] The fifth aspect of the present invention provides a cycloolefin ring-opening polymer, wherein the cycloolefin ring-opening polymer is prepared from the cycloolefin monomer according to any one of claims 1 to 3 and 8; wherein the structure of the cycloolefin ring-opening polymer is as shown in Formula II:

[0021]

[0022] In formula II,

[0023] m is 0, 1 or 2;

[0024] R represents an aromatic hydrocarbon substituent or an azaaryl group.

[0025] A sixth aspect of the present invention provides a method for preparing a cycloolefin ring-opening polymer, the preparation method comprising the following steps:

[0026] (1) subjecting the aforementioned cycloolefin monomer to a ring-opening metathesis polymerization reaction in an inert solvent in the presence of a catalyst to obtain an unsaturated cyclic polymer;

[0027] (2) In the presence of a hydrogenation catalyst, the unsaturated cyclic polymer is subjected to a hydrogenation reduction reaction to obtain the cycloolefin ring-opening polymer.

[0028] A seventh aspect of the present invention provides the use of the aforementioned cycloolefin ring-opening polymer in optical lenses, medical packaging materials or OLED light-emitting materials.

[0029] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0030] (1) The cycloolefin monomer provided by the present invention is a norbornene derivative containing a condensed aromatic hydrocarbon substituent. Compared with norbornene without a substituent or alkyl substituted, after the introduction of the condensed aromatic hydrocarbon group, the cycloolefin monomer has greater steric hindrance and rigidity, and the homopolymer will exhibit a higher glass transition temperature and better heat resistance.

[0031] (2) The cycloolefin monomer of the present invention can be used to prepare cycloolefin ring-opening polymers. The cycloolefin ring-opening polymers have the advantages of high glass transition temperature, high heat resistance, high refractive index and easy processing, and are suitable for preparing molding materials for optical elements such as optical lenses of smartphones and microscopes, and light guide plates of liquid crystal screens. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the product obtained in Preparation Example 2 of the present invention;

[0033] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of the product obtained in Preparation Example 5 of the present invention. DETAILED DESCRIPTION

[0034] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0035] The first aspect of the present invention provides a cycloolefin monomer, the structure of which is shown in Formula I:

[0036]

[0037] In Formula I,

[0038] L is 0, 1 or 2;

[0039] Ar represents an aromatic hydrocarbon substituent or an azaaryl group.

[0040] In the present invention, when L=0, it is a norbornene compound, when L=1, it is a tetracyclododecene compound, and when L=2, it is a trimer of norbornene and cyclopentadiene.

[0041] The cycloolefin monomer provided by the present invention is a norbornene derivative containing a condensed aromatic hydrocarbon substituent. Compared with norbornene without a substituent or alkyl-substituted, after the condensed aromatic hydrocarbon group is introduced, the cycloolefin monomer has greater steric hindrance and rigidity, and the homopolymer will show a higher glass transition temperature and better heat resistance.

[0042] In some embodiments of the present invention, the aromatic hydrocarbon substituent is selected from phenyl, aryl-substituted phenyl, naphthyl, anthracenyl, biphenyl or substituted aryl, preferably C12-C18 aryl-substituted phenyl, C10-C18 naphthyl, C14-C30 anthracenyl or C12-C24 biphenyl, more preferably C12-C16 naphthyl, C16-C22 anthracenyl.

[0043] In some embodiments of the present invention, the nitrogen heteroaryl group is selected from carbazole or β-carboline, preferably carbazole.

[0044] In some embodiments of the present invention, the cycloolefin monomer is a norbornene derivative.

[0045] Furthermore, the cycloolefin monomer is selected from at least one of the compounds having structures shown in Formulas I-1 to I-21:

[0046]

[0047]

[0048]

[0049] A second aspect of the present invention provides a method for preparing a cycloolefin monomer, wherein the preparation method comprises the following steps:

[0050] Under the protection of an inert gas, a diene and a dienophile are reacted in a solvent to obtain the cycloolefin monomer; wherein the structure of the cycloolefin monomer is as shown in Formula I:

[0051]

[0052] In Formula I,

[0053] L is 0, 1 or 2;

[0054] Ar represents an aromatic hydrocarbon substituent or an azaaryl group.

[0055] In some embodiments of the present invention, the diene is selected from cyclopentadiene compounds.

[0056] Furthermore, the cyclopentadiene compound is cyclopentadiene (CPD) or dicyclopentadiene (DCPD).

[0057] In some embodiments of the present invention, the dienophile is ethylene containing an aromatic hydrocarbon substituent.

[0058] Furthermore, the aryl substituent is an aromatic hydrocarbon substituent or an azaaryl group.

[0059] In some embodiments of the present invention, the dienophile is selected from at least one of the compounds having the structures shown in Formulae II-1 to II-9;

[0060]

[0061] In the present invention, those skilled in the art can obtain the dienophile by commercial purchase or by using existing techniques. The existing techniques generally use a Heck coupling reaction, for example, the reaction steps shown in Formula III:

[0062]

[0063] In some embodiments of the present invention, the molar ratio of the dienol to the dienophile is 1:1-3, for example, 1:1, 1:1.2, 1.1.5, 1.1.6, 1:1.7, 1:1.8, 1:1.9, 1.2, 1:2.2, 1:2.5, 1:2.8, 1:3 and any value in the range consisting of any two values, preferably 1:1.5-2.

[0064] In some embodiments of the present invention, the solvent is selected from benzene, toluene, xylene or tetrahydrofuran; preferably toluene.

[0065] In the preparation method of the present invention, after the reaction is completed, a first polymerization inhibitor is added, the obtained reaction liquid is filtered, and then the filter cake obtained by filtration is separated by column chromatography.

[0066] In some embodiments of the present invention, the first polymerization inhibitor is selected from 1,1-diphenyl-2-picrylhydrazyl (DPPH), ethyl vinyl ether or 2,2,6,6-tetramethylpiperidinyl nitroxide free radical; preferably 2,2,6,6-tetramethylpiperidinyl nitroxide free radical.

[0067] Furthermore, the addition amount of the first polymerization inhibitor is 0.5-1 mol% of the diene, such as 0.5 mol%, 0.6 mol%, 0.7 mol%, 0.8 mol%, 0.9 mol%, 1 mol% and any value in the range of any two values, preferably 0.6-0.8 mol%.

[0068] In some embodiments of the present invention, the reaction is a Diels-Alder reaction; the reaction conditions include: reaction pressure of 0.2-20 MPa, preferably 5-10 MPa; reaction temperature of 90-200° C., preferably 90-150° C.; reaction time of 0.5-3 h, preferably 1-2 h.

[0069] The third aspect of the present invention provides a cycloolefin monomer obtained by the aforementioned preparation method.

[0070] A fourth aspect of the present invention provides use of the aforementioned cycloolefin monomer in the preparation of an optical resin.

[0071] The COP resin prepared by using the monomer represented by formula I of the present invention has a better refractive index and transparency than the COP resin prepared by conventional norbornene monomers and commercially available COP resins, such as APEL and ZEONEX.

[0072] Compared with conventional norbornene monomers, the polycyclic aromatic hydrocarbon-substituted norbornene compounds provided by the present invention have greater steric hindrance and rigidity. The homopolymer prepared using the monomers of the present invention has a higher glass transition temperature, better heat resistance, and a high refractive index, and is suitable for preparing molding materials for optical elements such as high-end optical lenses and light guide plates of liquid crystal screens.

[0073] The fifth aspect of the present invention provides a cycloolefin ring-opening polymer, wherein the cycloolefin ring-opening polymer is prepared from the above-mentioned cycloolefin monomer; wherein the structure of the cycloolefin ring-opening polymer is as shown in Formula II:

[0074]

[0075] In formula II,

[0076] m is 0, 1 or 2;

[0077] R represents an aromatic hydrocarbon substituent or an azaaryl group.

[0078] The aryl-substituted norbornene monomer involved in the present invention can be used alone or in combination with monomers such as norbornene and dicyclopentadiene. It is preferred to use monomer I-1 or I-14 alone for polymerization.

[0079] In some embodiments of the present invention, the cycloolefin ring-opening polymer has a weight average molecular weight of 72000-84000 g / mol, a glass transition temperature of 170° C.-200° C., a refractive index of 1.52-1.54, and a light transmittance of 90-92%.

[0080] The cycloolefin ring-opening polymer material prepared from the cycloolefin monomer of the present invention has the advantages of high refractive index, high heat resistance, easy processing and the like.

[0081] A sixth aspect of the present invention provides a method for preparing a cycloolefin ring-opening polymer, the preparation method comprising the following steps:

[0082] (1) subjecting the aforementioned cycloolefin monomer to a ring-opening metathesis polymerization reaction in an inert solvent in the presence of a catalyst to obtain an unsaturated cyclic polymer;

[0083] (2) In the presence of a hydrogenation catalyst, the unsaturated cyclic polymer is subjected to a hydrogenation reduction reaction to obtain the cycloolefin ring-opening polymer.

[0084] In the present invention, the method for preparing the hydrogenated product of the cyclic olefin ring-opening polymer is not particularly limited, and reference is made to the methods described in, for example, Acc. Chem. Res. 2001, 34, 18-29, Angew. Chem. Int. Ed. 2006, 45, 3760-3765. Specifically, the method for preparing the cyclic olefin ring-opening polymer comprises the following steps: in the presence of a Hoveyda-Grubbs catalyst, a norbornene monomer is subjected to ring-opening metathesis polymerization in a toluene solution to obtain a cyclic olefin ring-opening polymer having syndiotacticity, and then the ring-opening polymer is subjected to hydrogenation reduction to obtain a hydrogenated product of the cyclic olefin ring-opening polymer.

[0085] In the present invention, the structure of the cycloolefin monomer is as shown in Formula I. Preferably, the cycloolefin monomer is selected from at least one of the compounds having structures shown in Formulas I-1 to I-21.

[0086] In some embodiments of the present invention, the catalyst is selected from the Hoveyda-Grubbs catalyst, such as (1,3-bis-(2,4,6-trimethylphenyl)-2-imidazolidinylidene)dichloro(o-isopropoxybenzylidene)ruthenium or dichloro(o-isopropoxyphenylmethylene)(tricyclohexylphosphine)ruthenium.

[0087] In some embodiments of the present invention, the amount of the catalyst added is 0.05-0.1 mol% of the cycloolefin monomer, for example, 0.05 mol%, 0.06 mol%, 0.07 mol%, 0.08 mol%, 0.09 mol%, 0.1 mol% and any value in the range of any two values, preferably 0.06-0.08 mol%.

[0088] In the preparation method of the present invention, after the ring-opening metathesis polymerization reaction is completed, a second polymerization inhibitor is also added. Preferably, the second polymerization inhibitor is selected from 1,1-diphenyl-2-picrylhydrazyl (DPPH), 2,2,6,6-tetramethylpiperidinyl nitroxide free radical or ethyl vinyl ether.

[0089] Furthermore, the added amount of the second polymerization inhibitor is 0.5-1 mol% of the cycloolefin monomer.

[0090] In some embodiments of the present invention, the pressure of the ring-opening metathesis polymerization reaction is 0.1 MPa-2 MPa, the temperature is 40° C.-80° C., and the time is 0.5-4 h.

[0091] In some embodiments of the present invention, the hydrogenation catalyst is selected from a heterogeneous catalyst supported on palladium, platinum or palladium.

[0092] In some embodiments of the present invention, the amount of the hydrogenation catalyst added is 5-10 mol% of the unsaturated cyclic polymer, such as 5 mol%, 6 mol%, 7 mol%, 8 mol%, 9 mol%, 10 mol% and any value in the range of any two values, preferably 6-8 mol%.

[0093] In some embodiments of the present invention, the hydrogenation reduction reaction is carried out under a pressure of 8 MPa-12 MPa, at a temperature of 80° C.-140° C., and for a time of 3-8 h.

[0094] In the present invention, the hydrogenation reduction reaction is carried out in an autoclave.

[0095] A seventh aspect of the present invention provides the use of the aforementioned cycloolefin ring-opening polymer in optical lenses, medical packaging materials or OLED light-emitting materials.

[0096] The cycloolefin ring-opening polymer prepared from the cycloolefin monomer of the present invention has the advantages of high glass transition temperature, high heat resistance, high refractive index and easy processing, and is suitable for preparing molding materials for optical elements such as optical lenses of smart phones and microscopes and light guide plates of liquid crystal screens.

[0097] In the present invention, the analytical test method is as follows:

[0098] The target monomer was analyzed using a nuclear magnetic resonance instrument, and the model of the nuclear magnetic resonance instrument was Bruker AVANCEⅢ500MHz.

[0099] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the hydrogenated product of cyclic olefin ring-opening polymer were analyzed using a Waters 410 volume gel exclusion chromatograph, using 6-chlorobenzene as the mobile phase, the mobile phase flow rate was 1.00 ml / min, and the test temperature was 110°C.

[0100] The glass transition temperature (Tg) of the hydrogenated product of the cyclic olefin ring-opening polymer was analyzed using a Mettler Toledo DSC821e differential scanning calorimeter produced by Mettler Company, and the test sample was measured at a heating rate of 10°C / min.

[0101] The refractive index of the hydrogenated product of cyclic olefin ring-opening polymer was analyzed using a KPR-200 precision refractometer produced by Shimadzu Corporation. The light sources were He lamp (587.6 nm) and H2 lamp (656.3 nm, 486.1 nm), and the test temperature was 25°C.

[0102] The transmittance of the hydrogenated product of the cyclic olefin ring-opening polymer was analyzed using a UV-2600I ultraviolet-visible spectrophotometer produced by Shimadzu Corporation, with an optical path length of 3 mm and a measuring wavelength of 650 nm.

[0103] The effects and effects of the method of the present invention are specifically described below in conjunction with embodiments, but the following embodiments do not constitute a limitation to the scheme of the present invention.

[0104] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0105] Preparation Example 1

[0106] The preparation method of 2-(bicyclo[2.2.1]hept-5-ene-2-yl)-6-phenylnaphthalene specifically comprises the following steps:

[0107] 2-phenyl-6-vinylnaphthalene (2.45 mol, 563 g) and 500 mL toluene were added to a 3 L autoclave, and the air in the autoclave was replaced with nitrogen; cyclopentadiene (1.3 mol, 86 g) was dissolved in 300 mL toluene solution, and then slowly added to the 3 L autoclave under nitrogen protection, and then heated to 150 ° C, maintaining the pressure at about 10 MPa, and the reaction was stopped for 2 hours. Heating was stopped and the inhibitor 2,2,6,6-tetramethylpiperidinyl nitroxide free radical (12.9 mol, 2 g) was added. The reaction solution was cooled to room temperature and filtered, and the filter cake was separated by column chromatography to obtain a white solid, i.e., 2-(bicyclo[2.2.1]hept-5-ene-2-yl)-6-phenylnaphthalene, with a yield of 68%.

[0108] The structural formula of 2-(bicyclo[2.2.1]hept-5-en-2-yl)-6-phenylnaphthalene is as follows:

[0109]

[0110] 1 H NMR (500MHz, Chloroform-d): δ7.99(1H,s),7.92(1H,s),7.68–7.61(3H,m),7.54(2H,d,J=13.0Hz),7.38–7.31(4H,m),5.90(2H,d,J=1.5Hz),3.13( 1H,s),2.69(1H,d,J=1.1Hz),2.34(1H,d,J=1.1Hz),2.03(1H,d,J=13.0Hz ), 1.97 (1H, d, J = 13.0Hz), 1.68 (1H, d, J = 13.0Hz), 1.63 (1H, d, J = 13.0Hz).

[0111] Preparation Example 2

[0112] The preparation method of 9-(bicyclo[2.2.1]hept-5-en-2-yl)-9H-carbazole specifically comprises the following steps:

[0113] N-vinyl carbazole (2.45 mol, 472 g) and 500 mL toluene were added to a 3 L autoclave, and the air in the autoclave was replaced with nitrogen; cyclopentadiene (1.3 mol, 86 g) was dissolved in 300 mL toluene solution, and then slowly added to the 3 L autoclave under nitrogen protection, and then the temperature was raised to 160 ° C and the pressure was maintained at about 10 MPa. After the reaction was stopped for 2 hours, the polymerization inhibitor 2,2,6,6-tetramethylpiperidinyl nitroxide free radical (12.9 mol, 2 g) was added. The reaction solution was cooled to room temperature and filtered, and the filter cake was separated by column chromatography to obtain a white solid, i.e., 9-(bicyclo[2.2.1]hept-5-ene-2-yl)-9H-carbazole, with a yield of 68%.

[0114] The structural formula of 9-(bicyclo[2.2.1]hept-5-en-2-yl)-9H-carbazole is as follows:

[0115]

[0116] The H NMR spectrum of this product is shown in Figure 1 .

[0117] 1H NMR (500MHz, Chloroform-d): δ7.99(2H,s),7.95(2H,d,J=0.7Hz),7.90(1H,s),7.60(1H,s),7.52(1H,s),7.40(1H,s),7.32(1H,s),5.89(2H, d,J=1.5Hz), 3.16(1H,s), 2.50(1H,d,J=1.0Hz), 2.34(1H,d,J=1.1Hz), 2.03(1H,d,J=13.0Hz), 1.95(1H,d,J=13.0Hz), 1.68(2H,d,J=2.6Hz).

[0118] Preparation Example 3

[0119] The preparation method of 3-(bicyclo[2.2.1]hept-5-en-2-yl)-9-phenyl-9H-carbazole specifically comprises the following steps:

[0120] 6-vinyl 9-phenyl-9H-carbazole (2.45 mol, 821 g) and 500 mL toluene were added to a 3 L autoclave, and the air in the autoclave was replaced with nitrogen; cyclopentadiene (1.3 mol, 86 g) was dissolved in 350 mL toluene solution, and then slowly added to the 3 L autoclave under nitrogen protection, and then the temperature was raised to 160 ° C and the pressure was maintained at about 10 MPa. After the reaction was stopped for 2 hours, the polymerization inhibitor 2,2,6,6-tetramethylpiperidinyl nitroxide free radical (12.9 mol, 2 g) was added. The reaction solution was cooled to room temperature and filtered, and the filter cake was separated by column chromatography to obtain an off-white solid, namely 3-(bicyclo[2.2.1]hept-5-ene-2-yl)-9-phenyl-9H-carbazole, with a yield of 67%.

[0121] The structural formula of 3-(bicyclo[2.2.1]hept-5-en-2-yl)-9-phenyl-9H-carbazole is as follows:

[0122]

[0123] 1 H NMR (500MHz, Chloroform-d): δ7.93(1H,s),7.78(1H,s),7.50–7.32(7H,m),7.30(1H,s),7.20(1H,s),7.16(1H,s),5.90(2H,d,J=4 .0Hz), 3.11(1H,s), 2.61(1H,d,J=1.0Hz), 2.17(1H,d,J=1.0Hz), 1.99(1H,d,J=13.0Hz), 1.89(1H,d,J=13.0Hz), 1.75–1.66(2H,m).

[0124] Preparation Example 4

[0125] The preparation method of 2-(6-phenylnaphthalene-2-yl)-1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalene specifically comprises the following steps:

[0126] 2-(Bicyclo[2.2.1]hept-5-ene-2-yl)-6-phenylnaphthalene (2mol, 724g) and 500mL toluene were added to a 3L autoclave, and the air in the autoclave was replaced with nitrogen; cyclopentadiene (1.2mol, 79.2g) was dissolved in 300mL toluene solution, and then slowly added to the 3L autoclave under nitrogen protection, and then the temperature was raised to 120°C, the pressure was maintained at about 6MPa, and the reaction was stopped after 2h. The polymerization inhibitor 2,2,6,6-tetramethylpiperidinyl nitroxide free radical (11.8mol, 1.84g) was added. The reaction solution was cooled to room temperature and filtered, and the filter cake was separated by column chromatography to obtain a white solid, i.e., 2-(6-phenylnaphthalene-2-yl)-1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalene, with a yield of 37%.

[0127] The structural formula of 2-(6-phenylnaphthalene-2-yl)-1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalene is as follows:

[0128]

[0129] 1 H NMR(500MHz,Chloroform-d): δ8.03(1H,s),8.00–7.94(2H,m),7.66–7.60(2H,m),7.5 5(1H,s),7.48–7.40(3H,m),7.40–7.33(1H,m),7.26(1H,s),5.90(2H,d,J=6.6Hz),2.9 1(1H,s),2.71(1H,d,J=0.9Hz),2.42–2.38(2H,m),2.28(2H,d,J=3.1Hz),2.12(1H,s) ,1.80–1.69(2H,m),1.46(1H,d,J=13.0Hz),1.40–1.32(2H,m),1.19(1H,d,J=13.0Hz).

[0130] Preparation Example 5

[0131] The preparation method of 9-(1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalene-2-yl)-9H-carbazole specifically comprises the following steps:

[0132] 9-(Bicyclo[2.2.1]hept-5-ene-2-yl)-9H-carbazole (1.8 mol, 466 g) and 500 mL toluene were added to a 3 L autoclave, and the air in the autoclave was replaced with nitrogen; cyclopentadiene (1 mol, 67 g) was dissolved in 300 mL toluene solution, and then slowly added to the 3 L autoclave under nitrogen protection, and then the temperature was raised to 130 ° C and the pressure was maintained at about 6 MPa. After reacting for 2 hours, the heating was stopped and the polymerization inhibitor 2,2,6,6-tetramethylpiperidinyl nitroxide free radical (9.8 mol, 1.53 g) was added. The reaction solution was cooled to room temperature and filtered, and the filter cake was separated by column chromatography to obtain a white solid, namely 9-(1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalen-2-yl)-9H-carbazole, with a yield of 41%.

[0133] The structural formula of 9-(1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalene-2-yl)-9H-carbazole is as follows:

[0134]

[0135] The H NMR spectrum of this product is shown in Figure 2 .

[0136] 1 H NMR (500MHz, Chloroform-d): δ7.94(2H,s),7.34(2H,s),7.18(4H,d,J=17.8Hz),5.90(2H,d,J=6.6Hz),4.39(1H,s),2.60(1H,d,J=0.9Hz),2.36–2.2 8(3H,m),2.25(1H,s),2.11(1H,s),1.93(1H,d,J=13.0Hz),1.76–1.68(2H , m), 1.37 (1H, d, J = 13.0Hz), 1.27 (1H, d, J = 13.0Hz), 1.21 (1H, d, J = 13.0Hz.

[0137] Example 1

[0138] (1) Under a nitrogen atmosphere, 150 g of the 2-(bicyclo[2.2.1]hept-5-en-2-yl)-6-phenylnaphthalene monomer obtained in Preparation Example 1 and 100 mL of toluene were added to a three-necked flask, mixed and stirred evenly, and the temperature of the reaction system was controlled to be 10° C.; 0.1 g of the Hoveyda-Grubbs catalyst was dissolved in 20 mL of toluene, and then the toluene solution of the catalyst was added dropwise to the reaction flask, and the temperature of the reaction system was controlled not to exceed 20° C. After the addition was completed, the reaction was stirred for 1 hour, 0.5 g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical was added, and the stirring was continued for 0.5 hour to obtain a cyclic olefin ring-opening metathesis polymer solution;

[0139] (2) The prepared polymer solution and 0.15g of ruthenium catalyst were added to a high-pressure reactor, hydrogen was introduced to a reaction pressure of 10MPa, and the reaction was carried out at 100°C for 6h. After the reaction was completed, 10% hydrogen peroxide solution was added to the system, and the catalyst was removed by filtration after standing. The residue was added to 1L of isopropanol and filtered to obtain a white polymer. Under vacuum conditions, it was dried at 40°C for 24 hours to obtain 106g of hydrogenated polymer with a yield of 91%. The number average molecular weight Mn was 25100g / mol, the weight average molecular weight Mw was 74000g / mol, and the transmittance, glass transition temperature and refractive index were shown in Table 1.

[0140] Example 2

[0141] (1) Under nitrogen atmosphere, 100 g of 9-(bicyclo[2.2.1]hept-5-en-2-yl)-9H-carbazole monomer prepared in Preparation Example 2 and 100 mL of toluene were added to a three-necked flask, mixed and stirred evenly, and the temperature of the reaction system was controlled to be 10° C. 0.08 g of Hoveyda-Grubbs catalyst was dissolved in 20 mL of toluene, and then the toluene solution of the catalyst was added dropwise to the reaction flask, and the temperature of the reaction system was controlled not to exceed 20° C. After the addition was completed, the reaction was stirred for 1 h, 0.3 g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical was added, and the stirring was continued for 0.5 h to obtain a cyclic olefin ring-opening metathesis polymer solution;

[0142] (2) The polymer solution and 0.1 g of ruthenium catalyst were added to a high-pressure reactor, hydrogen was introduced until the reaction pressure reached 10 MPa, and the reaction was carried out at 100°C for 6 h. After the reaction was completed, 10% aqueous hydrogen peroxide solution was added to the system, and the catalyst was removed by filtration after standing. The residue was added to 1 L of isopropanol and filtered to obtain a white polymer. The polymer was dried at 40°C for 24 h under vacuum conditions to obtain 80 g of hydrogenated polymer with a yield of 89%. The number average molecular weight Mn was 29800 g / mol; the weight average molecular weight Mw was 72300 g / mol. The transmittance, glass transition temperature and refractive index are shown in Table 1.

[0143] Example 3

[0144] (1) Under nitrogen atmosphere, 180 g of 3-(bicyclo[2.2.1]hept-5-en-2-yl)-9-phenyl-9H-carbazole monomer prepared in Preparation Example 3 and 200 mL of toluene were added to a three-necked flask, mixed and stirred evenly, and the temperature of the reaction system was controlled to be 10° C. 0.12 g of Hoveyda-Grubbs catalyst was dissolved in 20 mL of toluene, and then the toluene solution of the catalyst was added dropwise to the reaction flask, and the temperature of the reaction system was controlled not to exceed 20° C. After the addition was completed, the reaction was stirred for 1 h, 0.6 g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical was added, and the stirring was continued for 0.5 h to obtain a cyclic olefin ring-opening metathesis polymer solution.

[0145] (2) The polymer solution and 0.18g of ruthenium catalyst were added to a high-pressure reactor, hydrogen was introduced to a reaction pressure of 10MPa, and the reaction was carried out at 100°C for 6h. After the reaction was completed, 10% hydrogen peroxide solution was added to the system, and the catalyst was removed by filtration after standing. The residue was added to 1L of isopropanol and filtered to obtain a white polymer. Under vacuum conditions, it was dried at 40°C for 24 hours to obtain 120g of hydrogenated polymer with a yield of 86%. The number average molecular weight Mn was 30800g / mol; the weight average molecular weight Mw was 73400g / mol, and the transmittance, glass transition temperature and refractive index were shown in Table 1.

[0146] Example 4

[0147] (1) Under nitrogen atmosphere, 80 g of 2-(6-phenylnaphthalene-2-yl)-1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalene monomer prepared in Preparation Example 4 and 100 mL of toluene were added to a three-necked flask, mixed and stirred evenly, and the temperature of the reaction system was controlled to be 10° C. 0.06 g of Hoveyda-Grubbs catalyst was dissolved in 20 mL of toluene, and then the toluene solution of the catalyst was added dropwise to the reaction flask, and the temperature of the reaction system was controlled not to exceed 20° C. After the addition was completed, the reaction was stirred for 1 hour, 0.2 g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical was added, and stirring was continued for 0.5 hour to obtain a cyclic olefin ring-opening metathesis polymer solution;

[0148] (2) The polymer solution and 0.1 g of ruthenium catalyst were added to a high-pressure reactor, hydrogen was introduced until the reaction pressure reached 10 MPa, and the reaction was carried out at 100°C for 6 h. After the reaction was completed, 10% aqueous hydrogen peroxide solution was added to the system, and the catalyst was removed by filtration after standing. The residue was added to 1 L of isopropanol and filtered to obtain a white polymer. The polymer was dried at 40°C for 24 h under vacuum conditions to obtain 75 g of hydrogenated polymer with a yield of 83%. The number average molecular weight Mn was 36800 g / mol; the weight average molecular weight Mw was 81000 g / mol. The transmittance, glass transition temperature and refractive index are shown in Table 1.

[0149] Example 5

[0150] (1) Under nitrogen atmosphere, 100 g of 9-(1,2,3,4,4a,5,8,8a-octahydro-1,4:5,8-dimethylnaphthalene-2-yl)-9H-carbazole prepared in Preparation Example 5 and 200 mL of toluene were added to a three-necked flask, mixed and stirred evenly, and the temperature of the reaction system was controlled to be 10°C. 0.12 g of Hoveyda-Grubbs catalyst was dissolved in 20 mL of toluene, and then the toluene solution of the catalyst was added dropwise to the reaction flask, and the temperature of the reaction system was controlled not to exceed 20°C. After the addition was completed, the reaction was stirred for 1 hour, 0.6 g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical was added, and the stirring was continued for 0.5 hour to obtain a cyclic olefin ring-opening metathesis polymer solution.

[0151] (2) The polymer solution and 0.18g of ruthenium catalyst were added to a high-pressure reactor, hydrogen was introduced until the reaction pressure reached 10MPa, and the reaction was carried out at 100°C for 6h. After the reaction was completed, 10% aqueous hydrogen peroxide solution was added to the system, and the catalyst was removed by filtration after standing. The residue was added to 1L of isopropanol and filtered to obtain a white polymer. Under vacuum conditions, it was dried at 40°C for 24 hours to obtain 120g of hydrogenated polymer with a yield of 80%. The number average molecular weight Mn was 38800g / mol; the weight average molecular weight Mw was 83500g / mol, and the transmittance, glass transition temperature and refractive index were shown in Table 1.

[0152] Comparative Example 1

[0153] Under nitrogen atmosphere, 500g of norbornene and 350mL of toluene were added to a three-necked flask, mixed and stirred evenly, and the temperature of the reaction system was controlled to be 10°C. 0.23g of Hoveyda-Grubbs catalyst was dissolved in 50mL of toluene, and then the toluene solution of the catalyst was added dropwise to the reaction flask, and the temperature of the reaction system was controlled not to exceed 20°C. After the addition was completed, the reaction was stirred for 1h, 2.6g of 2,2,6,6-tetramethylpiperidinyl nitroxide free radical was added, and the stirring was continued for 0.5h to obtain a cyclic olefin ring-opening metathesis polymer solution. The polymer solution and 0.5g of ruthenium catalyst were added to a high-pressure reactor, hydrogen was introduced to the reaction pressure of 10MPa, and the reaction was carried out at 100°C for 6h. After the reaction was completed, 10% aqueous hydrogen peroxide solution was added to the system, and the catalyst was removed by filtration after standing. The residue was added to 3L of isopropanol, and a white polymer was obtained after filtration. Under vacuum conditions, it was dried at 40°C for 24 hours to obtain 430g of hydrogenated polymer with a yield of 93%. The number average molecular weight Mn is 18100; the weight average molecular weight Mw is 38010. The transmittance, glass transition temperature and refractive index are shown in Table 1.

[0154] Comparative Example 2

[0155] The hydrogenated product of the cyclic olefin ring-opening polymer in this comparative example is JSR ARTON, purchased from JSR Corporation of Japan. The transmittance, glass transition temperature and refractive index are shown in Table 1.

[0156] Comparative Example 3

[0157] The hydrogenated product of the cyclic olefin ring-opening polymer in this comparative example is ZEONEX 330R, purchased from Zeon Corporation of Japan. The transmittance, glass transition temperature and refractive index are shown in Table 1.

[0158] Table 1 Physical and chemical properties test results of Examples 1-5 and Comparative Examples 1-3

[0159] project Mn,g / mol Mw,g / mol Tg / ℃ Refractive Index Light transmittance / % Example 1 25100 74000 180 1.534 92% Example 2 29800 72300 188 1.534 92% Example 3 30800 73400 173 1.526 92% Example 4 36800 81000 195 1.528 91% Example 5 38800 83500 190 1.530 91% Comparative Example 1 18100 38010 110 1.505 90% Comparative Example 2 - - 165 1.513 91% Comparative Example 3 - - 123 1.509 91%

[0160] As can be seen from Table 1, the ring-opening polymers prepared using aromatic substituted norbornene monomers in Examples 1, 2, and 3 have a lower weight average molecular weight than the ring-opening polymers prepared using aromatic substituted tetracyclododecene monomers in Examples 4 and 5, but have higher glass transition temperatures, refractive indices, and better light transmittance.

[0161] The ring-opening polymers prepared using aromatic-substituted norbornene monomers in Examples 1, 2 and 3 have higher glass transition temperatures, refractive indices and better light transmittance than the ring-opening polymers prepared using unsubstituted and alkyl-substituted norbornene monomers in Comparative Examples 1 and 2.

[0162] The ring-opening polymers prepared using aromatic-substituted norbornene monomers in Examples 1, 2 and 3 have higher glass transition temperatures, higher refractive indices and better light transmittance than the commercially available ring-opening polymers in Comparative Examples 2 and 3.

[0163] As can be seen from the above, the hydrogenated ring-opening metathesis cycloolefin polymer synthesized using the monomers described in the present invention has a glass transition temperature, refractive index and light transmittance that are better than those of the hydrogenated ring-opening metathesis cycloolefin polymer prepared using conventional norbornene monomers.

[0164] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A cycloolefin monomer, It is characterized in that The structure of the cycloolefin monomer is shown in Formula I: In Formula I, L is 0, 1 or 2; Ar represents an aromatic hydrocarbon substituent or an azaaryl group.

2. The cycloolefin monomer according to claim 1, in, The aromatic hydrocarbon substituent is selected from phenyl, aryl-substituted phenyl, naphthyl, anthracenyl, biphenyl or substituted aryl, preferably C12-C18 aryl-substituted phenyl, C10-C18 naphthyl, C14-C30 anthracenyl or C12-C24 biphenyl; And / or, the nitrogen heteroaryl group is selected from carbazole or β-carboline, preferably carbazole.

3. The cycloolefin monomer according to claim 1 or 2, in, The cycloolefin monomer is a norbornene derivative; Preferably, the cycloolefin monomer is selected from at least one of the compounds having the structures shown in Formulas I-1 to I-21:

4. A method for preparing a cycloolefin monomer, It is characterized in that The preparation method comprises: Under the protection of an inert gas, a dien, a dienophile and a first polymerization inhibitor are reacted in a solvent to obtain the cycloolefin monomer; wherein the structure of the cycloolefin monomer is as shown in Formula I: In Formula I, L is 0, 1 or 2; Ar represents an aromatic hydrocarbon substituent or an azaaryl group.

5. The preparation method according to claim 4, in, The diene is selected from cyclopentadiene compounds; preferably, the cyclopentadiene compound is cyclopentadiene or dicyclopentadiene; And / or, the dienophile is ethylene containing an aromatic substituent; preferably, the aromatic substituent is an aromatic substituent or an azaaryl; more preferably, the dienophile is at least one selected from the compounds having the structures shown in formula II-1 to II-9; And / or, the first polymerization inhibitor is selected from 1,1-diphenyl-2-picrylhydrazyl (DPPH), ethyl vinyl ether or 2,2,6,6-tetramethylpiperidinyl nitroxide free radical; preferably 2,2,6,6-tetramethylpiperidinyl nitroxide free radical; And / or, the solvent is selected from benzene, toluene, xylene or tetrahydrofuran.

6. The preparation method according to claim 4 or 5, in, The molar ratio of the diene to the dienophile is 1:1-3; preferably 1:1.5-2; And / or, the amount of the first polymerization inhibitor added is 0.5-1 mol% of the cycloolefin monomer.

7. The preparation method according to any one of claims 4 to 6, in, The reaction is a Diels-Alder reaction; the reaction conditions include: reaction pressure of 0.2MPa-20MPa, reaction temperature of 90°C-200°C, and reaction time of 0.5-3h.

8. Cycloolefin monomer obtained by the preparation method according to any one of claims 4 to 7.

9. Use of the cycloolefin monomer according to any one of claims 1 to 3 and 8 in the preparation of optical resins.

10. A cycloolefin ring-opening polymer, It is characterized in that The cycloolefin ring-opening polymer is prepared from the cycloolefin monomer according to any one of claims 1 to 3 and 8; wherein the structure of the cycloolefin ring-opening polymer is as shown in Formula II: In formula II, m is 0, 1 or 2; R represents an aromatic hydrocarbon substituent or an azaaryl group.

11. The cycloolefin ring-opening polymer according to claim 10, in, The cycloolefin ring-opening polymer has a weight average molecular weight of 72000-84000 g / mol, a glass transition temperature of 170° C.-200° C., a refractive index of 1.52-1.54, and a light transmittance of 90-92%.

12. A method for preparing a cycloolefin ring-opening polymer, It is characterized in that The preparation method comprises the following steps: (1) subjecting the cycloolefin monomer according to any one of claims 1 to 3 and 8 to a ring-opening metathesis polymerization reaction in an inert solvent in the presence of a catalyst, and adding a second polymerization inhibitor to obtain an unsaturated cyclic polymer; (2) In the presence of a hydrogenation catalyst, the unsaturated cyclic polymer is subjected to a hydrogenation reduction reaction to obtain the cycloolefin ring-opening polymer.

13. The preparation method according to claim 12, in, The catalyst is selected from the group consisting of Hoveyda-Grubbs catalyst; and / or, the catalyst is added in an amount of 0.05-0.1 mol% of the cycloolefin monomer; and / or, the second polymerization inhibitor is selected from 1,1-diphenyl-2-picrylhydrazyl (DPPH), ethyl vinyl ether or 2,2,6,6-tetramethylpiperidinyl nitroxide free radical; preferably 2,2,6,6-tetramethylpiperidinyl nitroxide free radical; and / or, the amount of the second polymerization inhibitor added is 0.5-1 mol% of the cycloolefin monomer; And / or, the ring-opening metathesis polymerization reaction is carried out under a pressure of 0.1 MPa-2 MPa, a temperature of 40° C.-80° C., and a time of 0.5-4 h.

14. The preparation method according to claim 12 or 13, in, The hydrogenation catalyst is selected from a heterogeneous catalyst supported by palladium, platinum or palladium; and / or, the amount of the hydrogenation catalyst added is 5-10 mol% of the unsaturated cyclic polymer; And / or, the hydrogenation reduction reaction is carried out under a pressure of 8 MPa-12 MPa, a temperature of 80° C.-140° C., and a time of 3-8 h.

15. Use of the cycloolefin ring-opening polymer according to claim 10 or 11 or the cycloolefin ring-opening polymer prepared by the preparation method according to any one of claims 12 to 14 in optical lenses, medical packaging materials or OLED light-emitting materials.

Citation Information

Cited By

  • Cycloolefin copolymer and preparation method thereof

    CN119798616A