Method for extracting high-purity ortho-, meta-and para-phenol from mixed cresol

Through the extraction of high-purity paraphenol from mixed cresol by decomposing and distillation technology, the problem of extraction of high-purity cresol in the existing technology is solved, the production cost is reduced, and product performance and market competitiveness are improved.

CN119059885APending Publication Date: 2024-12-03YANCHENG INST OF TECH

Patent Information

Application Number
CN202411173831.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently extract high-purity orthopara phenol from mixed cresol, resulting in high production costs of photoresist and phenolic resins, and the impurity content affects product performance.

Method used

Using impurity removal and distillation technology, the impurities such as 2,6-dicresol, 2,4-dicresol, etc. that affect the synthesis of phenolic resins are removed from mixed cresols, and the reaction of o-cresol and o-ethyl phenol with formaldehyde is used. Instead of partial paracresol, improve the purity and utilization of m-p-cresol and reduce production costs.

Benefits of technology

The extraction of high-purity intero-parameter phenols has been achieved, the production costs of photoresist and phenolic resins have been reduced, the scope of application of crude phenols has been expanded, and the product variety and market competitiveness have been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010131600000111
    Figure BDA0005010131600000111
  • Figure BDA0005010131600000121
    Figure BDA0005010131600000121
  • Figure BDA0005010131600000131
    Figure BDA0005010131600000131
Patent Text Reader

Abstract

The invention relates to a method for extracting high-purity ortho-m-para-phenol from mixed cresol, which comprises the following steps of: adding the mixed cresol into a stirring reaction kettle, sampling and analyzing the content of aniline and organic acid in the mixed cresol, adding a medicament for treatment according to the analysis condition, adding the treated mixed cresol into a tower kettle of a high-efficiency rectifying tower, and performing reflux dehydration to obtain the high-purity ortho-m-para-phenol. And supplementing concentrated sulfuric acid which accounts for 0-1% of the mass of the mixed cresol, and rectifying at the top of the tower at the same time. According to the method, 2, 6-xylenol, 2, 4-xylenol and other impurities influencing phenolic resin synthesis in mixed cresol are removed through rectification, high-purity ortho-m-p-phenol is obtained and can be used for synthesizing m-cresol-phenolic resin for photoresist, and therefore the source of photoresist raw materials is increased, and the synthesis cost is reduced. According to different raw materials, more than 98% of o-cresol / p-cresol mixture, p-cresol / o-ethyl phenol mixture, crude p-cresol and the like can be produced as by-products, and the method is simple and easy to implement, high in additional value and remarkable in economic benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for extracting high-purity o-meta-para phenol from mixed cresols, belonging to the technical field of organic separation. Background Art

[0002] Industrial para-cresol is made from crude phenol in the refining workshop of a coking enterprise. After distillation, phenol, o-cresol, meta-cresol, and industrial xylenol are obtained, with meta-cresol being one of the products. Meta-cresol is widely used in the synthesis of phenolic resins and modified phenolic resins, such as 2126#, 1681#, 284# phenolic resins, 211# rosin-modified phenolic resins, etc.; it is used as a raw material for organophosphorus insecticides cypermethrin, insecticides cypermethrin, and pyrethroids chlorfenapyr in pesticides; meta-cresol can be used as a disinfectant and preservative; in addition, meta-cresol is also used as a raw material for dyes, fragrances, resins, and color films. Para-cresol is used as a raw material for the antioxidant 2,6-di-tert-butyl-p-methylphenol, and can also be used in synthetic resins, paints, plasticizers, pesticides, and medicines.

[0003] Meta-cresol formaldehyde resin has very good performance and can be used on the substrate for photoresist as a special resin. For a long time, due to the relatively high content of impurities such as phenol, 2,6-dimethylphenol, 2,4-dimethylphenol, naphthalene, and aniline in meta-cresol, the performance of products using meta-cresol as raw material has been affected, such as the weather resistance, oxidation resistance, and anti-aging performance of synthetic resins have all been reduced. It is necessary to improve the quality of meta-cresol and reduce the impurity content, especially to increase the content of ortho-meta-paraphenol. At the same time, due to the high price of high-purity meta-cresol, the production cost is also high. Therefore, by selecting suitable cresol raw materials (i.e., mixed cresols) and using distillation to prepare high-purity ortho-meta-paraphenol (mixed content of more than 99%), the content of phenol, 2,6-dimethylphenol, 2,4-dimethylphenol, naphthalene, and aniline can be easily controlled to below 0.1%, providing raw material guarantee for the production of meta-cresol formaldehyde resin photoresist.

[0004] The raw materials of mixed cresols include crude phenol from coal gasification, crude phenol from coking or crude phenol from water, etc., and crude phenol extracted from gasified and pyrolyzed coal tar. The content of each component in the mixed cresol obtained by distillation of crude phenol from gasification, coking cresol, crude phenol from water, etc. is usually: o-cresol 0-80%, m-p-cresol 10-97%, o-ethylphenol 0-3%, phenol 0-20%, 2,4 / 2,5-xylenol 0-10%, 2,6-xylenol 0-2%, naphthalene 0-1%, aniline 0-2%, valeric acid 0-1%. The mixed cresols obtained by extracting crude phenol from gasified and pyrolyzed coal tar and distilling it usually have the following contents: o-cresol 0-80%, m-p-cresol 10-91%, o-ethylphenol 0-15%, phenol 0-5%, 2,4 / 2,5-xylenol 0-25%, 2,6-xylenol 0-15%, naphthalene 0-1%, aniline 0-2%, and valeric acid 0-1%. The contents of o-cresol, 2,6-xylenol, o-ethylphenol, p-cresol, 2,4-xylenol, 2,5-xylenol, etc. in crude phenol extracted from gasified and pyrolyzed coal tar are usually much higher than those in crude phenol from coking, crude phenol from coal gasification, crude phenol in water, etc., which affects the extraction of 99% m-cresol (in production, only crude phenol from coking can mass-produce 99% m-cresol, and crude phenol from gasification can only produce m-cresol of grades below 98%). It is much easier to collect 99-100% o-cresol / m-cresol / o-ethylphenol products instead. Currently, basically all crude phenol raw materials can be produced (more suitable for pyrolyzed coal tar phenol), with low production cost and high competitiveness.

[0005] The activity of various phenols in reacting with formaldehyde varies greatly (the activity of phenol in reacting with formaldehyde is defined as 1), m-cresol is 2.88, while p-cresol (0.31), o-cresol (0.26), and o-ethylphenol (0.28). Therefore, in synthesizing m-cresol-formaldehyde resin with m-cresol, the performance of o-cresol and o-ethylphenol partially replacing p-cresol to synthesize phenolic resin is almost the same. They are all linear segments for producing phenolic resin, which is equivalent to replacing 99-100% of the expensive m-cresol to synthesize m-cresol-formaldehyde resin. Since there are appropriate numbers of p-cresol, o-cresol, and o-ethylphenol units in the resin chain, the resin also has good linearity and good flexibility, and is particularly suitable for the electronics industry as a film material for photoresist. The processing performance, heat resistance, and electrical properties of this phenolic resin are significantly better than those of the phenolic resin synthesized with phenol.

[0006] Since impurities in the raw material m-cresol will affect the quality of m-cresol-formaldehyde resin, there are requirements for the content of various impurities. The functionality of phenol in the reaction with formaldehyde is 3, the same as m-cresol. The presence of phenol will change the structure and properties of m-cresol-formaldehyde resin (the heat resistance of the resin will decrease, and the resin will change color and deteriorate when dehydrated at high temperature). Therefore, the phenol content in high-purity o-m-para-phenol should be as small as possible; the functionality of 2,4-xylenol and 2,6-xylenol in the reaction with formaldehyde is 1, and only 6-hydroxymethyl-2,4-xylenol, 4-hydroxymethyl-2,6-xylenol and their condensation products can be generated, and no The presence of a small amount of xylenol can improve the heat resistance of the resin, but due to the end-capping effect, the resin chain will be broken to form a small molecular weight resin, which will cause the risk of widening the molecular weight distribution and decreasing the resin performance. Therefore, the 2,4 / 2,5-xylenol and 2,6-xylenol in the high-purity o-m-para-phenol used for synthesis should be as small as possible; the presence of o-ethylphenol and o-cresol will not affect the performance of m-cresol-formaldehyde resin. The activity of o-ethylphenol and o-cresol is similar to that of p-cresol, and the functionality is 2. They also react with formaldehyde to form linear resins, which has little effect on the resin performance.

[0007] The Chinese invention patent with publication number CN101602837A discloses a method for preparing phenolic resin for wire enamel: dissolving polyformaldehyde with distilled water at a temperature range of 70 to 80°C, adding m-p-cresol and weak base and stirring, heating to 95 to 98°C, keeping warm until emulsification, adding weak acid for neutralization after emulsification for 1 to 3 hours, and stopping heating; vacuum dehydrating the solution obtained in the above steps, with the removal of water, the temperature drops, and heating is started when the vacuum degree is ≥0.095Mpa, water is continuously removed, the color of the solution changes from turbid to transparent, and the temperature rises by 5 to 10°C after transparency, and heating is stopped; adding a phenolic solvent to the resin solution obtained in the above steps, dissolving, and obtaining the desired product. The meta-cresol raw material has a meta-cresol content of 45-50%. The composition of such meta-cresol is approximately: 45-50% meta-cresol, 30-35% para-cresol, 7-10% o-cresol, 1-3% o-ethylphenol, 5-15% 2,4 / 2,5-xylenol, 1-5% 2,6-xylenol, etc. Such raw materials react with formaldehyde to produce products such as 4-hydroxymethyl-2,6-xylenol, 2-hydroxymethyl-4,6-xylenol, 4-hydroxymethyl-2-methyl-6-ethylphenol, etc. These products cannot continue to react with formaldehyde to form a polycondensate phenolic resin, and can only condense two molecules to form a dihydric phenol. The molecular weight of this dihydric phenol is relatively low (more than 200), which has a greater impact on the performance of the phenolic resin. Therefore, this meta-cresol (the product name on the market is 45% meta-cresol) is used. The sulfur and nitrogen content of this meta-cresol is 0.1% or even higher, and it cannot be used for high-grade phenol Production of phenolic resin; however, the raw materials for the production of wire enamel contain dibasic or tribasic acid anhydrides, dibasic or tribasic alcohols or phenols, which react to form polyesters; dihydric phenols generated by the dehydration condensation of two molecules of 4-hydroxymethyl-2,6-dimethylphenol, 2-hydroxymethyl-4,6-dimethylphenol, and 4-hydroxymethyl-2-methyl-6-ethylphenol, this dihydric phenol or 4-hydroxymethyl-2,6-dimethylphenol, 2-hydroxymethyl-4,6-dimethylphenol, 4-hydroxymethyl-2-methyl-6-ethylphenol can replace dibasic or tribasic alcohols to react with acid anhydrides to form polyesters with better performance, and have little effect on wire enamels, so m-p-cresol containing part of 2,6-dimethylphenol and 2,4-dimethylphenol can be used for resins for wire enamels, but this 45% m-p-cresol is not suitable for the production of other phenolic resins with higher requirements, and cannot be used for the synthesis of phenolic resins for the production of high-grade photoresists.

[0008] Chinese invention patents with publication numbers CN103289718A and CN 106543389 A both introduce processes for preparing phenolic resins from phenol-containing coal tar. The difference between patent CN106543389 A and patent CN103289718A is that toluene or benzene is added as a solvent, an acid or a base is used as a catalyst, coal tar or its distillation fraction undergoes a phenolic polymerization reaction with formaldehyde, benzaldehyde, polyformaldehyde and furfural under certain conditions, and the reaction product is filtered through a closed drum vacuum filter to obtain a phenolic resin, and at the same time, dephenolized coal tar containing a solvent is obtained. The reaction of this type of inventive phenol mixture with aldehydes has the following problems: first, 2,4-dimethylphenol, 2,6-dimethylphenol, 6-ethyl-2-methylphenol, 2,3,6-trimethylphenol, 2,4,5-trimethylphenol, 2,4,6-trimethylphenol, 2,4-methylethylphenol, etc. can only obtain condensation products when reacting with aldehydes, and cannot be further polycondensed to obtain polymer phenolic resins; second, trimethylphenol has a high freezing point, and the viscosity is large when synthesizing phenolic resins, and the reaction cannot be guaranteed to be complete; third, it is very difficult to separate the phenolic resin from the dephenolized phenol oil and water after synthesis, and phenolic resins of certain specifications cannot be obtained. The resin has a high oil content, low molecular weight, and an unexpectedly high free phenol content. When the resin is used, water and low-boiling substances will be released, resulting in poor quality of downstream products. Except for being used in low-end products such as flower mud, it has few other practical uses. Moreover, due to the high low volatile matter, free phenol and free aldehyde content, it is very unfriendly to the environment and occupational protection.

[0009] The Chinese invention patent with application number 202111105969.1 provides a phenolic resin for photoresist, which is prepared by polycondensation of the following raw materials: p-cresol, m-cresol, xylenol, 3,3'-dimethyl-4,4'-biphenol, 2-hydroxy-1-hydroxymethylnaphthalene, spirodiphenol, formaldehyde and / or polyformaldehyde. A certain amount of 3,3'-dimethyl-4,4'-biphenol, spirodiphenol and 2-hydroxy-1-hydroxymethylnaphthalene are added to the photoresist phenolic resin, and the three play a synergistic role within a certain proportion range, so that the heat resistance of the obtained phenolic resin, as well as the resolution and photosensitivity of the photoresist are improved at the same time. The invention prepares phenolic resin with a three-stage production process. By controlling the process conditions such as the feeding order, reaction temperature, and time, a phenolic resin with excellent comprehensive performance is obtained. After testing, its softening temperature is about 136°C and the molecular weight distribution is narrow. As a film-forming resin for photoresist, it has excellent performance. The cresols are p-cresol and m-cresol; the xylenols are selected from at least one of 2,4-xylenol, 2,6-xylenol, 2,5-xylenol, 3,5-xylenol and 3,4-xylenol. The p-cresol, m-cresol and xylenol used in the comparative document are basically petrochemical grade products with high product prices and high production costs; and the selected xylenols contain 2,6-xylenol and 2,4-xylenol (functionality is 1), which cannot be polycondensed with formaldehyde to form phenolic resins, but can only produce dimers, which will seriously affect the degree of polymerization and molecular weight distribution of phenolic resins, thereby affecting the resin properties.

[0010] The Chinese invention patent with application number 202211664332.0 discloses a phenolic resin and a photoresist. The phenolic resin includes a product formed by the condensation of a specified phenol with an aldehyde. The specified phenol includes a first type of phenol and a second type of phenol. The second type of phenol includes at least one of cresol, xylenol and trimethylol. The photoresist includes the above-mentioned phenolic resin, which can effectively improve the photosensitivity of the photoresist while maintaining good heat resistance and morphology of the photoresist. Regarding the second type of phenol, cresol refers to a phenol with a methyl group substituted on the benzene ring, which can include one or more of o-cresol, m-cresol and p-cresol; xylenol refers to a phenol with two methyl groups substituted on the benzene ring, which can include 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol and 3,5-xylenol; trimethylphenol refers to a phenol with three methyl groups substituted on the benzene ring, which can include one or more of 2,3,5-trimethylphenol, 2,3,6-trimethylphenol, 2,4,5-trimethylphenol, 2,4,6-trimethylphenol and 3,4,5-trimethylphenol. The second-class phenols used in this patent, namely, p-cresol, m-cresol, xylenol and tri-cresol, are basically petrochemical-grade products. The raw materials of the first-class phenols and the second-class phenols are expensive and the production costs are high. In addition, the selected xylenols contain 2,6-xylenol, 2,4-xylenol, 2,3,6-tri-cresol, 2,4,5-tri-cresol and 2,4,6-tri-cresol (with a functionality of 1 or 0). These xylenols and tri-cresols either do not react with formaldehyde or cannot be polycondensed to form phenolic resins, and can only produce dimers, which will seriously affect the degree of polymerization and molecular weight distribution of the phenolic resin, thereby affecting the resin properties.

[0011] The Chinese invention patent with publication number CN116333239 A discloses a linear high molecular weight xylenol phenolic resin and its preparation and utilization, wherein the phenols are one or more of 3,5-xylenol, xylenol, m-cresol, and p-cresol; the aldehydes are one or more of formaldehyde, acetaldehyde, salicylaldehyde, and furfural; and the acid catalyst is one or more of hydrochloric acid, oxalic acid, acetic acid, sulfuric acid, and nitric acid. The cresols used in the examples are only pure m-cresol and p-cresol; the xylenol used is only 3,5-xylenol, and no other xylenols and ethylphenol are used. The raw material composition requirements are high, the price is high, and the production is difficult. It is impossible to extract high-purity m-p-cresol from coal crude phenol, so the application field is narrow. Summary of the invention

[0012] The present invention aims to solve the above-mentioned shortcomings and provide a method for extracting high-purity o-para-phenol from mixed cresols. The mixed cresol used in the method has a wide source, a wide range of applications, is easy to produce and purify, and has a very low price. The present invention uses impurity removal and distillation to remove 2,6-xylenol, 2,4-xylenol, and 6-ethyl-2-cresol from the mixed cresols that affect the synthesis of phenolic resins, thereby obtaining phenol, mixed phenols, meta-para-cresol and other raw materials (2,6-xylenol, 2,4-xylenol, and 6-ethyl-2-cresol) different from those used in the traditional phenolic resin synthesis. , 4-xylenol and 6-ethyl-2-cresol have low contents, generally required to be ≤0.5%, and raw materials for photoresist ≤0.1%), and the reaction activity of o-cresol, o-ethylphenol and formaldehyde is similar to that of p-cresol, and o-cresol and o-ethylphenol are used to replace part of p-cresol, and m-p-cresol with high ortho-content is used to replace 99% of petrochemical m-p-cresol and formaldehyde to produce m-cresol aldehyde resin for photoresist, thereby increasing the source of raw materials for producing photoresist and reducing the cost of synthesizing photoresist. While producing photoresist, the present invention can also produce more than 98% of o-cresol / p-cresol mixture, p-cresol / o-ethylphenol mixture, o-cresol / p-cresol / o-ethylphenol mixture, crude p-cresol, etc. according to different raw materials, and can further obtain pure o-cresol, p-cresol, o-ethylphenol and other products. The method is simple and easy to operate, has high added value, better process operability, stronger practicality, excellent safety, and significant economic benefits.

[0013] To achieve the above object, the present invention adopts the following technical solution:

[0014] A method for extracting high-purity o-meta-para-phenol from mixed cresols: adding the mixed cresols into a stirred reactor, sampling and analyzing the contents of aniline and organic acid in the mixed cresols, adding a reagent for treatment according to the analysis results, adding the treated mixed cresols into the reactor of a high-efficiency distillation tower, reflux dehydration, adding 0.01-1% concentrated sulfuric acid of the mass of the mixed cresols to continue oxidation and impurity removal, and simultaneously performing vacuum distillation at the top of the tower to obtain high-purity o-meta-para-phenol with a content of 99%;

[0015] The high-purity o-para-p-phenol with a content of 99% is used as a raw material to synthesize the m-cresol-formaldehyde resin for photoresist;

[0016] The mixed cresols are derived from crude phenol from coal gasification, crude phenol from coking, crude phenol in water or crude phenol extracted from gasified and pyrolyzed coal tar.

[0017] The content of each component in the mixed cresol is: 0-80% of o-cresol, 10-98% of m-p-cresol / o-ethylphenol, 0-20% of phenol, 0-20% of 2,4 / 2,5-xylenol, 0-20% of 2,6-xylenol, 0-1% of naphthalene, 0-2% of aniline, and 0-1% of valeric acid; preferably: 10-80% of o-cresol, 20-90% of m-p-cresol / o-ethylphenol, 0-5% of phenol, 0-5% of 2,4 / 2,5-xylenol, 0-1.0% of 2,6-xylenol, 0-0.5% of naphthalene, 0-0.5% of aniline, and 0-0.5% of valeric acid.

[0018] Furthermore, the adding of reagents for treatment according to the analysis results is specifically as follows: if the content of organic acid in the mixed cresol is higher than that of aniline, the added reagent is 1 to 1.5 times the molar amount of sodium bicarbonate of the organic acid; if the content of aniline in the mixed cresol is higher than that of organic acid, the added reagent is 1 to 1.5 times the molar amount of sulfuric acid of the aniline; if the molar amount of aniline to the organic acid is (0.95 to 1.05):1, the added reagent is 0.5 to 1.0 times the molar amount of sulfuric acid of the aniline.

[0019] Furthermore, the number of theoretical plates of the high-efficiency distillation tower is 200-350.

[0020] Furthermore, the reflux ratio of the vacuum distillation is 5 to 30, preferably 15 to 20, and the pressure of the vacuum distillation is -0.05 to -0.1 MPa.

[0021] Furthermore, when the mixed cresols are derived from crude phenol from coal gasification, crude phenol from coking or crude phenol from water, after distillation, in addition to obtaining high-purity o-meta-para-phenol with a content of 99%, the following fractions are also obtained: 95% phenol, a mixed phenol fraction with o-cresol ≤ 20%, a mixed phenol fraction with an o-cresol content of 20% to 50%, an o-cresol-enriched fraction, 99.5% o-cresol, and an o-cresol post-fraction containing 2,6-dimethylphenol; wherein 95% phenol, o-cresol ≤ 20 % of the mixed phenol fraction and the mixed phenol fraction with an o-cresol content of 20% to 50% are used to produce phenolic resin; the o-cresol enriched fraction is re-distilled to prepare 99.5% o-cresol; 99.5% o-cresol is used to produce o-cresol epoxy phenolic resin for electronic plastic packaging and pesticide 2-methyl-4-chlorophenol; the o-cresol post-fraction containing 2,6-dimethylphenol is used to produce 35% cresol for wire enamel, or to produce o-methyl anisole and 2,6-dimethyl anisole;

[0022] When the mixed cresols are derived from crude phenol extracted from gasified and pyrolyzed coal tar, after distillation, in addition to obtaining high-purity o-meta-paraphenol with a content of 99%, the following fractions are also obtained: a phenol / o-cresol fraction with an o-cresol content of ≤20%, a mixed phenol fraction with an o-cresol content of 20% to 50%, an o-cresol-enriched fraction, 99.5% o-cresol, an o-cresol / 2,6-xylenol fraction, and a crude 2,4 / 2,5-xylenol product; Among them, the phenol / o-cresol fraction with o-cresol ≤ 20% and the mixed phenol fraction with o-cresol content of 20% to 50% are used to produce phenolic resin; the o-cresol enriched fraction is re-distilled to prepare 99.5% o-cresol; the o-cresol / 2,6-xylenol fraction is used to separate and produce pure 2,6-xylenol; the crude 2,4 / 2,5-xylenol is used to separate and produce 6-tert-butyl-2,4-xylenol and 99% 2,5-xylenol.

[0023] Method for producing phenolic resin using these fractions:

[0024] 1) Thermosetting resin (insulation materials, refractory materials, flower mud, etc.)

[0025] Ⅰ. Phenolic raw materials are 95% phenol, mixed phenol fraction with o-cresol ≤ 20%, and phenol / o-cresol fraction with o-cresol ≤ 20%:

[0026] Start stirring, add phenolic raw materials (one or more of 95% phenol, mixed phenol fraction with o-cresol ≤ 20%, phenol / o-cresol fraction with o-cresol ≤ 20%) into the reactor, the amount added is 60-100% of the phenolic raw materials; then add alkali (the flake alkali can be dissolved in a small amount of water, the amount of alkali is 0.5-5% of the phenol), raise the temperature to about 50-55°C, turn off the steam, slowly raise the temperature to 70-75°C, turn on the cooling water, add or drop formaldehyde or polyformaldehyde in batches for reaction (the amount of aldehyde is 1.1-1.5 of the molar amount of phenol), the dropping time is 2-3 hours, add the remaining phenolic raw materials after dropping, keep the temperature for reaction for 1-3 hours, and pay more attention to observing the temperature changes of the materials before and after turning on and off the steam and cooling water.

[0027] After the reaction is finished, add medium or weak acid to neutralize to neutrality, maintain for more than 10 minutes, re-test the pH value and pass it, turn on the vacuum pump, start dehydration, observe that the dehydration speed slows down or until the temperature drops to about 70-75°C, turn on steam heating, and during dehydration, constantly adjust the steam switch according to the speed of water output to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at about 80°C. When the water level reaches the required value (about 80% of the mass of phenolic materials, the actual value is subject to production data), take samples to analyze the moisture and viscosity, stop vacuuming when the moisture is 2-3%, and add an appropriate amount of ethylene glycol to condition the viscosity (the viscosity is higher than 20Pa.s, and then use ethanol to adjust the viscosity), adjust the viscosity to the specified value of 15-20Pa.s, cool to 50°C and discharge.

[0028] Ⅱ. The phenolic raw materials are the mixed phenol fraction with an o-cresol content of 20% to 50% and the o-cresol enriched fraction:

[0029] Start stirring, add 60-100% of phenol raw materials (mixed phenol fraction with o-cresol content of 20%-50% and / or o-cresol enriched fraction) into the reactor; add alkali (the flake alkali can be dissolved in a small amount of water, and the amount of alkali is 0.5-5% of phenol), raise the temperature to about 50-55°C, turn off the steam, slowly raise the temperature to 70-75°C, turn on the cooling water, add or drop formaldehyde or polyformaldehyde in batches to react (the amount of aldehyde is 1.1-1.5 of the molar amount of phenol), the dropping time is 2-3 hours, and after dropping, add the remaining phenol raw materials, keep the temperature for reaction for 1-3 hours, and pay more attention to observing the temperature changes of the materials before and after turning on and off the steam and cooling water.

[0030] After the reaction is finished, add a medium or weak acid to neutralize to neutrality, maintain for more than 10 minutes, retest the pH to be qualified, turn on the vacuum pump, start dehydration, observe that the dehydration speed slows down or until the temperature drops to about 70-75°C, turn on steam heating, and during dehydration, the steam switch should be continuously adjusted according to the speed of water discharge to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at about 80°C. When the water level is dehydrated to the required value (about 80% of the mass of phenolic materials, the actual value is subject to production data), sample and analyze the moisture and viscosity. When the moisture is 2-3%, stop vacuuming, add an appropriate amount of ethylene glycol to adjust the viscosity (the viscosity is higher than 20Pa.s, and then use ethanol to adjust the viscosity), adjust the viscosity to the specified value of 15-20Pa.s, cool to 50°C and discharge;

[0031] The evaporated water is allowed to stand and separate into layers. The crude o-cresol in the lower layer is reused or refined o-cresol, and the water layer is reused (when the aldehyde is paraformaldehyde) or sent to the wastewater treatment section for treatment.

[0032] 2) Thermoplastic resins (refractory materials, friction materials, brake pads, bakelite, etc.)

[0033] Ⅰ. Phenolic raw materials are 95% phenol, mixed phenol fraction with o-cresol ≤ 20%, and phenol / o-cresol fraction with o-cresol ≤ 20%:

[0034] a) Liquid resin

[0035] Start stirring, add 60-100% of phenol raw materials (95% phenol, mixed phenol fraction with o-cresol ≤20%, phenol / o-cresol fraction with o-cresol ≤20%), add oxalic acid or oxalic acid / phosphoric acid mixture (dissolved in appropriate amount of water, oxalic acid:phosphoric acid = 0-10:0-1, 0.1-3% of the weight of phenol), formaldehyde (partial formaldehyde, the total amount of formaldehyde is 0.65-0.95 of the molar amount of phenol).

[0036] After the feeding is completed, use pH test paper to determine the pH of the reaction liquid to be 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate is strictly controlled within 1-3℃ / min. The rate is determined to be 1.5-2.5℃ / min to avoid heating too fast, which will cause the reaction liquid to bubble out and affect the resin quality.

[0037] Raise the temperature to 95°C and start the heat preservation reaction. The reaction temperature is controlled at 95-100°C and stabilized at 98-99°C. Keep the temperature for 1-3 hours. Then, add the remaining formaldehyde and phenolic raw materials dropwise after about 1 hour to continue the reaction. During the reaction, pay close attention to the whitening time. Add hydrochloric acid after 0.5 hours of whitening, continue the heat preservation reaction for 1 hour, and add alkali (dissolved in appropriate amount of water) to neutralize after judging the reaction end point.

[0038] When the pH value of the neutralization reaction liquid is determined to be 6.0-7.0 by test paper, adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally controlled at about 50% of the phenol feed amount, and the specific water level is based on the water level being constant within 20 minutes.

[0039] After confirming that dehydration is complete, add ethylene glycol to dilute. When the resin temperature drops to 78°C, add ethanol to dilute. After stirring for 0.5 hour, initially measure the viscosity. Finally, adjust to the required viscosity with the specified ratio of ethylene glycol to ethanol, stir for another hour, cool naturally, and discharge the material when the resin temperature is less than 70°C.

[0040] b) Solid resin

[0041] The production of solid resin is basically the same as above, except that after the white reaction is completed, no alkali is added for neutralization. The final dehydration temperature is directly controlled at 110-150°C, and the final pressure is controlled at -0.09-0.095Mpa to make the moisture content meet the requirements. The material is discharged into a stainless steel plate while hot, cooled, and then crushed or granulated directly with a granulator.

[0042] Ⅱ. The phenolic raw materials are the mixed phenol fraction with an o-cresol content of 20% to 50% and the o-cresol enriched fraction:

[0043] a) Liquid resin

[0044] Start stirring, add 60-100% of phenol raw materials (mixed phenol fraction with o-cresol content of 20%-50%, o-cresol enriched fraction) into the reactor; add oxalic acid or oxalic acid / phosphoric acid mixture (dissolved in appropriate amount of water, oxalic acid:phosphoric acid = 0-10:0-1, 0.1-3% of the weight of phenol), formaldehyde (partial formaldehyde, the total amount of formaldehyde is 0.65-0.95 of the molar amount of phenol).

[0045] After the feeding is completed, use pH test paper to determine the pH of the reaction liquid to be 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate should be strictly controlled within 1-3℃ / min to avoid heating too quickly, which will cause the reaction liquid to leak out and affect the resin quality.

[0046] The temperature was raised to 95°C and the reaction was started by heat preservation. The reaction temperature was controlled at 95-100°C and the reaction was carried out for 1-3 hours. Then, the remaining formaldehyde and phenol raw materials were added dropwise in about 1 hour to continue the reaction.

[0047] During the reaction, pay close attention to the whitening time. Add hydrochloric acid after 0.5 hour of whitening, continue to keep warm and react for 1 hour. After judging the reaction endpoint, add alkali (dissolved in appropriate amount of water) to neutralize.

[0048] When the pH value of the neutralization reaction liquid is determined to be 6.0-7.0 by test paper, adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally controlled at about 50% of the phenol feed amount, and the specific water level is based on the water level being constant within 20 minutes.

[0049] After confirming that dehydration is complete, add ethylene glycol to dilute. When the resin temperature drops to 78°C, add ethanol to dilute. After stirring for 0.5 hour, initially measure the viscosity. Finally, adjust to the required viscosity with the specified ratio of ethylene glycol to ethanol, stir for another hour, cool naturally, and discharge the material when the resin temperature is less than 70°C.

[0050] The evaporated water is allowed to stand and separate into layers. The crude o-cresol in the lower layer is reused or refined o-cresol, and the water layer is reused (when the aldehyde is paraformaldehyde) or sent to the wastewater treatment section for treatment.

[0051] b) Solid resin

[0052] The production of solid resin is basically the same as above, except that after the white reaction is completed, no alkali is added for neutralization. The final dehydration temperature is directly controlled at 110-150°C, and the final pressure is controlled at -0.09-0.095Mpa to make the moisture content meet the requirements. The material is discharged into a stainless steel plate while hot, cooled, and then crushed or granulated directly with a granulator.

[0053] Further, a method for synthesizing m-cresol-formaldehyde resin for photoresist using the high-purity o-m-para-phenol obtained by the above method comprises the following steps:

[0054] (1) adding high-purity ortho-para-phenol and an acidic catalyst into a reaction kettle, heating to 80° C., adding paraformaldehyde or formaldehyde in batches, heating to 95° C. to 100° C. at a heating rate of 1 to 3° C. / min after the addition, keeping the temperature for reaction for 2 to 4 hours, sampling and analyzing the cresol content in the reaction solution, and determining the content of cresols ≤ 0.5% as qualified. If the content is unqualified, adding a small amount of paraformaldehyde or formaldehyde and continuing the reaction until the content is qualified;

[0055] (2) The reaction liquid is heated to perform steam distillation. The evaporated gas is condensed in a reflux condenser and enters a water separator. The upper layer is water, which is refluxed into the reaction kettle for reuse. The lower layer is a mixed phenol of o-cresol / p-cresol / o-ethylphenol, which is collected in a collection tank. After there is no obvious oil in the evaporated condensate, piperidine acetate adduct is added to the reaction liquid and mixed. The vacuum device is adjusted and vacuum dehydration is started. The dehydration temperature is 80-85°C, the time is 2-3 hours, and the final pressure is controlled to -0.07 5~-0.08Mpa, while observing the water level of the receiver, based on the water level being constant within 20min, the collected water and the mixture of o-cresol / p-cresol / o-ethylphenol are respectively combined, the collected mixture of o-cresol / p-cresol / o-ethylphenol can be combined with high-purity o-meta-paraphenol to produce phenolic resin with high straight-chain structure, and can also be used to separate the raw materials for producing o-cresol, p-cresol and o-ethylphenol; the collected water can be partially used (to dissolve polyformaldehyde and increase the fluidity of the reaction materials), or sent to the three waste workshop for treatment;

[0056] (3) gradually increasing the vacuum degree to 0.098 MPa, further increasing the temperature for dehydration, and when the temperature of the material in the kettle reaches 190° C. and no liquid is distilled out, keeping the temperature for 1 hour, stopping the dehydration, and removing the vacuum with nitrogen. Under the protection of nitrogen, discharge the material while hot into a stainless steel plate, and after cooling, break it into pieces and bag it to obtain m-cresol-formaldehyde resin;

[0057] In step (1), the acidic catalyst is a mixture of oxalic acid and formic acid in a molar ratio of (2-8):(0.1-1), and the amount used is 0.5-5% of the mass of high-purity o-para-phenol;

[0058] In step (2), the preparation method of the piperidine acetate adduct is as follows: piperidine is added dropwise to glacial acetic acid in a mass ratio of 4:(5-11), the temperature is controlled to be lower than 50° C., and after mixing, the mixed solvent is recovered under reduced pressure to obtain the product.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] (1) The present invention provides a method for extracting high-purity o-para-phenol from mixed cresols. When crude phenol from coal gasification, crude phenol from coking or crude phenol in water is used as a raw material to purify the mixed cresols, the extracted high-purity o-para-phenol has a total content of o-cresol + m-para-cresol + o-ethylphenol of 99.0-100%, phenol ≤0.1%, 2,6-xylenol ≤0.1%, 2,4 / 2,5-xylenol ≤0.2%, aniline ≤0.1%, naphthalene ≤0.1%, and valeric acid ≤0.1%;

[0061] When crude phenol extracted from gasified and pyrolyzed phenol-containing coal tar is used as a raw material to purify mixed cresols, in the extracted high-purity o-para-o-cresol, the total content of o-para-cresol + o-ethylphenol is 99.0-100%, 2,6-dimethylphenol is ≤0.5%, 2,4 / 2,5-dimethylphenol is ≤0.5%, 6-ethyl-2-methylphenol is ≤0.1%, aniline is ≤10ppm, naphthalene is ≤0.1%, and valeric acid is ≤0.1%. Furthermore, the total content of o-para-cresol + o-ethylphenol is 99.5-100%, 2,6-dimethylphenol is ≤0.1%, 2,4 / 2,5-dimethylphenol is ≤0.2%, 6-ethyl-2-methylphenol is ≤0.05%, aniline is ≤1ppm, naphthalene is ≤0.01%, and valeric acid is ≤0.01%.

[0062] Since the allowable range of the content of o-cresol and o-ethylphenol in the high-purity o-para-phenol product of the present invention is much higher than that in pure m-para-cresol, the difficulty of distillation is greatly reduced, and the requirements for the efficiency of the distillation tower are significantly lower. Therefore, distillation is relatively easy and the distillation extraction cost is low.

[0063] (2) In the conventional method, due to the high content of o-ethylphenol, 2,6-dimethylphenol and 2,4-dimethylphenol in the crude phenol extracted from medium and low temperature tar, it is impossible to produce m-para-cresol of a grade of more than 95%, let alone m-para-cresol of more than 98%, thereby limiting the application scope of the crude phenol from tar. The method of the present invention allows a high content of o-ethylphenol, so the distillation process is applicable to crude phenol of various compositions, including crude phenol with a high o-ethylphenol content extracted from medium and low temperature tar, thereby expanding the application scope of the crude phenol and increasing the variety of products.

[0064] (3) The present invention extracts high-purity o-para-phenol from mixed cresols and uses the high-purity o-para-phenol as a raw material for m-cresol-formaldehyde resin for photoresist. The raw material price for synthesizing phenol-formaldehyde resin is cheaper than m-para-cresol and does not affect the performance of downstream products, thus being conducive to enhancing market competitiveness.

[0065] (4) The present invention can not only extract high-purity o-meta-para-phenol, but also obtain a mixed phenol fraction with an o-cresol content of 20% to 50%, which can be used to prepare phenolic resin products and produce crude o-cresol as a by-product.

[0066] (5) When the mixed cresols purified from crude phenol extracted from gasified and pyrolyzed coal tar are used as raw materials, the method of the present invention can also be used to extract o-cresol / 2,6-xylenol with a high 2,6-xylenol content, thereby further separating 2,6-xylenol and its derivatives.

[0067] (6) The high-purity ortho-para-phenol extracted by the present invention can be used to synthesize photoresist meta-cresol-formaldehyde resin. In the synthesis process, an acid-base amphoteric organic catalyst can be used to adjust the pH of the reaction solution by adjusting the amount of organic acid and organic base used, thereby adjusting and improving the molecular weight and molecular weight distribution, thereby improving the performance of the product.

[0068] (7) When crude phenol from coal gasification, crude phenol from coking or crude phenol from water is used as the mixed cresol raw material, the method of the present invention is used to obtain, in addition to obtaining high-purity o-meta-para-phenol with a content of 99%, the following fractions are obtained: 95% phenol, a mixed phenol fraction with o-cresol ≤ 20%, a mixed phenol fraction with an o-cresol content of 20% to 50%, an o-cresol-enriched fraction, 99.5% o-cresol, and an o-cresol post-fraction containing 2,6-dimethylphenol; wherein, 95% phenol, o-cresol ≤ 20% % of the mixed phenol fraction, and the mixed phenol fraction with an o-cresol content of 20% to 50% are used to produce phenolic resin; the o-cresol enriched fraction is re-distilled to prepare 99.5% o-cresol; 99.5% o-cresol is used to produce o-cresol epoxy phenolic resin for electronic plastic packaging and pesticide 2-methyl-4-chlorophenol; the o-cresol post fraction containing 2,6-xylenol is used to produce 35% cresol for enameled wire varnish, and can also be used to produce o-methyl anisole and 2,6-dimethyl anisole. 95% phenol, mixed phenol fraction with o-cresol ≤ 20%, and mixed phenol fraction with an o-cresol content of 20% to 50% and a 2,6-xylenol content of ≤ 0.1% are suitable for the synthesis of phenolic resin.

[0069] When crude phenol extracted from gasified and pyrolyzed coal tar is used as a mixed cresol raw material, the method of the present invention is adopted to obtain not only high-purity o-meta-paraphenol with a content of 99%, but also fractions: a phenol / o-cresol fraction with an o-cresol content of ≤20%, a mixed phenol fraction with an o-cresol content of 20% to 50%, an o-cresol-enriched fraction, 99.5% o-cresol, an o-cresol / 2,6-xylenol fraction, and a crude 2,4 / 2,5-xylenol product; Among them, the phenol / o-cresol fraction with o-cresol ≤ 20% and the mixed phenol fraction with o-cresol content of 20% to 50% are used to produce phenolic resin; the o-cresol enriched fraction is re-distilled to prepare 99.5% o-cresol; the o-cresol / 2,6-xylenol fraction is used to separate and produce pure 2,6-xylenol; the crude 2,4 / 2,5-xylenol is used to separate and produce 6-tert-butyl-2,4-xylenol and 99% 2,5-xylenol. The phenol / o-cresol fraction with o-cresol ≤ 20% and the mixed phenol fraction with o-cresol content of 20% to 50% have a 2,6-xylenol content of ≤0.1%; the o-cresol enriched fraction has a 2,6-xylenol content of ≤0.5%, which is suitable for the synthesis of phenolic resin.

[0070] (8) The mixture of phenol and o-cresol produced by the present invention that does not contain 2,6-dimethylphenol has a price of only 50-60% of petrochemical phenol. Therefore, the cost of synthesizing phenolic resin with low-content phenol and mixed phenol is more than 20% cheaper than commercially available phenolic resin. Using 10,000 tons of mixed phenol instead of phenol to synthesize phenolic resin can save about 25 million per year. DETAILED DESCRIPTION

[0071] The technical solution of the present invention is clearly and completely described below in conjunction with specific embodiments.

[0072] Example 1

[0073] A method for extracting high-purity o-meta-para-phenol from mixed cresols comprises: adding 10,000 parts of mixed cresols (derived from crude phenol extracted from phenol-containing coal tar, the mass percentage content of each component in the mixed cresols: 8.33% of phenol, 0.46% of 2,6-dimethylphenol, 0.52% of naphthalene, 0.05% of aniline, 0.42% of valeric acid, 71.28% of o-cresol, 15.26% of m-para-cresol, 3.62% of o-ethylphenol) into a stirred kettle, adding 40 parts of sodium bicarbonate, heating to 90°C and stirring for reaction for two hours, then transferring the material into a kettle of a rectification tower equipped with stainless steel packing, performing full reflux for 4 hours, and heating at -0.086MPa and a reflux ratio of 15 The mixture was distilled under reduced pressure under the conditions of 40:1~20:1, and samples were taken every hour to analyze the content of phenolic substances (to control 2,6-dimethylphenol and naphthalene). Then, 263.2 parts of 95.6% phenol, 584.8 parts of mixed phenols, 785.9 parts of o-cresol fraction, 5079.9 parts of 99.5% o-cresol, 600.1 parts of o-cresol post-fraction, 2411.3 parts of high-purity o-m-para-phenol (50.9% m- and p-cresol, including 32.7% m-cresol and 18.2% p-cresol) and 256.9 parts of kettle residue were collected in sequence, and samples were taken for chromatographic analysis respectively (the kettle residue contained sodium bicarbonate and sodium valeric acid salt, so the sample was distilled and then subjected to chromatographic analysis). The results of chromatographic analysis are shown in Table 1.

[0074] Table 1 Chromatographic analysis results

[0075]

[0076] Note: The ratio of high-purity o-para-phenol intermediate cresol: (o-cresol + o-ethylphenol + p-cresol) is 32.4:67.6; the mixed phenol (excluding 2,6-dimethylphenol and 2,4-dimethylphenol) obtained by combining the phenol section and the mixed phenol section can be used to replace phenol to synthesize phenolic resin.

[0077] The high-purity o-meta-para-phenol extracted in Example 1 does not contain 2,6-xylenol and 2,4-xylenol, and can be used to produce m-cresol-formaldehyde resin or high-grade phenolic resin for photoresist. Among other fractions, the phenol section (95% phenol) can be used to produce phenolic resin; the mixed phenol section can be used to extract petrochemical-grade phenol or produce phenolic resin; the o-cresol fraction section can be used to extract refined o-cresol; the refined o-cresol section can be used to produce o-cresol epoxy phenolic resin; the o-cresol post-fraction can be used to mix 35% cresol or 45% m-meta-cresol; after the still residue accumulates to a certain amount, it is rectified to extract high-purity o-meta-para-phenol or used to separate m-meta-cresol to produce m-cresol, o-ethylphenol, 6-tert-butyl-o-cresol, 2,6-di-tert-butyl-p-cresol, etc.

[0078] Example 2

[0079] A method for extracting high-purity o-m-para-phenol from mixed cresols: adding 10,000 parts of mixed cresols (derived from crude phenol extracted from phenol-containing coal tar, the mass percentage content of each component in the mixed cresol: 0.02% of 2,6-dimethylphenol, 0.02% of naphthalene, 0.32% of aniline, 8.96% of o-cresol, 71.37% of m-para-cresol, 16.95% of o-ethylphenol, 2.3% of 2,4 / 2,5-dimethylphenol) into an enamel stirring kettle, heating to 120°C, dripping 51.6 parts of 98% sulfuric acid under stirring, the dripping time is 1 hour, and the temperature is kept for reaction for 1 hour after the dripping is completed; then the material is transferred into the kettle of a rectification tower equipped with stainless steel fillers After reflux, 20 parts of 98% sulfuric acid were added dropwise, and the whole reflux was performed for 3 hours. Vacuum distillation was performed under the conditions of -0.086MPa and a reflux ratio of 15 to 20:1. Samples were taken every hour to analyze the content of phenolic substances (2,6-dimethylphenol and naphthalene should be controlled). Then, 9191.4 parts of 99.87% high-purity o-para-phenol (72.91% of m-para-cresol, including 46.84% of m-cresol and 26.07% of p-cresol), 526.3 parts of the post-m-para-cresol fraction, and 269.3 parts of the still residue (2,4 / 2,5-dimethylphenol-enriched materials, containing sulfuric acid and its derivatives) were collected in turn, and samples were taken for chromatographic analysis. The results of the chromatographic analysis are shown in Table 2.

[0080] Table 2 Chromatographic analysis results

[0081]

[0082] Among the above fractions, high-purity o-para-phenol can be used to produce meta-cresol-formaldehyde resin for photoresist, or sold as a product; the meta-cresol fraction can be used to mix 35% cresol and 45% meta-cresol to produce varnish for enameled wire, and the meta-cresol fraction can also be accumulated to a certain amount and then subjected to secondary distillation to extract high-purity o-para-phenol or used to separate meta-cresol to produce meta-cresol, o-ethylphenol, 2,6-di-tert-butyl-p-cresol, etc.; the still residue is used for further distillation to obtain more than 90% of 2,4 / 2,5-xylenol, preparing raw materials for the separation of 2,4 / 2,5-xylenol.

[0083] Example 3

[0084] A method for extracting high-purity o-meta-para-phenol from mixed cresols: adding 10,000 parts of mixed cresols (mixed cresols extracted from phenol-containing coal tar, with the mass percentage of each component being: 6.2% phenol, 5.3% 2,6-dimethylphenol, 0.31% naphthalene, 0.18% aniline, 31.6% o-cresol, 46.5% m-para-cresol, 4.38% o-ethylphenol, 4.8% 2,4 / 2,5-dimethylphenol, and 0.63% others) into a stirred kettle, adding 20 parts of sulfuric acid, heating to 90°C and stirring for reaction for two hours, then transferring the material into the kettle of a rectification tower equipped with stainless steel packing, performing full reflux for 2 hours, adding 20 parts of 98% sulfuric acid, and stirring at -0.086Mpa and a reflux ratio of 15 to 20. : 1 condition, sampling and analyzing the content of phenolic substances every 1 hour (to control 2,6-xylenol and naphthalene), then collecting in sequence 539.9 parts of phenol / o-cresol, 778.5 parts of o-cresol enriched fractions, 1229 parts of 99.57% o-cresol, 1531.3 parts of o-cresol / 2,6-xylenol fractions (o-cresol rear fractions), 5149.7 parts of 99.81% high-purity o-meta-paraphenol, 528.3 parts of 2,4 / 2,5-xylenol fractions, 125.8 parts of kettle residues (containing 36.3 parts of 2,4 / 2,5-xylenol), sampling for chromatographic analysis respectively (the kettle residue was subjected to chromatographic analysis after distillation of the sample because it contained sulfuric acid and its derivative phenolsulfonic acid), and the results of chromatographic analysis are shown in Table 3.

[0085] Table 3 Chromatographic analysis results

[0086]

[0087]

[0088] Among the above-collected fractions, the contents of 2,6-dimethylphenol and 2,4-dimethylphenol in high-purity o-para-phenol are both less than 0.1%, and the contents of aniline are only 1.3 ppm, which can be used to produce phenolic resin for photoresist; 2,6-dimethylphenol and 2,4-dimethylphenol were not detected in the phenol / o-cresol fraction and the o-cresol enriched fraction, which are relatively good raw materials for the synthesis of phenolic resin; refined o-cresol can be used to produce o-cresol epoxy phenolic resin, and the o-cresol / 2,6-dimethylphenol fraction can be used to separate 2,6-dimethylphenol; the 2,4 / 2,5-dimethylphenol enriched fraction can be used to purify and separate 2,4-dimethylphenol, etc.; the still residue is used to extract dimethylphenol.

[0089] Example 4

[0090] A method for extracting high-purity o-para-phenol from mixed cresols: 10,000 parts of mixed cresols (45% para-cresol obtained by gasification phenol extraction, mass percentage of each component: 3.2% phenol, 0.6% 2,6-dimethylphenol, 0.1% aniline, 7.5% o-cresol, 45.8% meta-cresol, 27.8% para-cresol, 0.6% o-ethylphenol, 9.6% 2,4 / 2,5-dimethylphenol, 3.1% 2,3-dimethylphenol, 0.8% para-ethylphenol, 0.9% others, 328ppm sulfur, The mixture was stirred for 1 hour at 90°C and then transferred into the kettle of a distillation tower equipped with stainless steel fillers, and refluxed for 2 hours. 20 parts of 98% sulfuric acid were added, and vacuum distillation was performed at -0.086MPa and a reflux ratio of 15 to 20:1. The phenol content was analyzed by sampling every hour (to control 2,6-dimethylphenol and naphthalene), and then 3195 parts of the first 35% cresols (316.8 parts of phenol, 104.7 parts of 2,6-dimethylphenol, 669 parts of o-cresol) were collected in sequence. .7 parts, p-cresol 788.2 parts, m-cresol 1298.2 parts, o-ethylphenol 17.4 parts), 4497.5 parts of 98.83% high-purity m-cresol (4.2 parts of 2,6-xylenol, 5.2 parts of o-cresol, 1698.6 parts of p-cresol, 2746.4 parts of m-cresol, 35.5 parts of o-ethylphenol, 4.1 parts of 2,4 / 2,5-xylenol, 2.8 parts of 2,3-xylenol, and 0.6 parts of others), 1840.7 parts of 35% cresol (295.4 parts of p-cresol, 489.6 parts of m-cresol, o-ethylphenol 6.4 parts of phenol, 836.9 parts of 2,4 / 2,5-dimethylphenol, 182.5 parts of 2,3-dimethylphenol, 25.7 parts of m-p-ethylphenol and 4.2 parts of others), 418.9 parts of kettle residue (containing 50 parts of sulfuric acid and its derivatives, 109.3 parts of 2,4 / 2,5-dimethylphenol, 121.6 parts of 2,3-dimethylphenol, 63.1 parts of m-p-ethylphenol and 74.9 parts of others), were sampled for chromatographic analysis respectively (the kettle residue contained sulfuric acid and its derivative phenolsulfonic acid, so the sample was distilled before chromatographic analysis), and the results of chromatographic analysis are shown in Table 4.

[0091] Table 4 Chromatographic analysis results

[0092]

[0093]

[0094] In Table 4, the 35% cresol product is obtained by collecting the first 35% cresol and the last 35% cresol of high-purity o-cresol / m-cresol by distillation, and can be used to produce wire enamel; high-purity o-m-cresol can be used to produce m-cresol-formaldehyde resin for photoresist; and the kettle residue can be used to extract mixed xylenols.

[0095] Example 5 (Preparation of thermosetting resin, mainly used as a binder for low-carbon and low-carbon magnesium-carbon bricks)

[0096] Add 263.2 parts of 95.6% phenol obtained in Example 1, 236.8 parts of mixed phenol (the mixed sample analysis shows 80.44% phenol, 19.19% o-cresol, and does not contain 2,6-dimethylphenol), 5 parts of caustic soda flakes (dissolved in 10 parts of water, 1% of the mass of phenol), and 185 parts of 37% formaldehyde in sequence in the reactor (the total molar ratio of formaldehyde to phenol is 1.37:1), heat to 40-45°C, turn off the steam, turn on the cooling water at 50-55°C, slowly heat to 80-85°C, and keep warm for 1 hour; add 200 parts of 37% formaldehyde dropwise for a second time, the addition time is 1 hour, and the heat is kept for 0.5 hour; then add the remaining 200 parts of 37% formaldehyde dropwise, the addition time is 1 hour, and the heat is kept for 1 hour after the dripping is completed. Pay more attention to the temperature change of the material before and after the steam and cooling water are turned on.

[0097] After the reaction is completed, add glacial acetic acid to neutralize to neutrality, maintain for 10 minutes, start the vacuum pump to evacuate, and start dehydration after the vacuum is stable. When the dehydration speed slows down or the temperature drops to 70-75°C, turn on the steam heating. During dehydration, the steam switch should be continuously adjusted according to the speed of water output to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at about 80°C. When the water level reaches the required value (420 parts, the actual value is subject to production data), samples are taken to analyze the moisture and viscosity. When the moisture is 2-3%, stop evacuation, and add ethylene glycol to adjust the viscosity to the specified value of 15-20Pa.s. After the viscosity reaches the requirement, cool down to 50°C and discharge 695 parts of the material, which is a brown-red transparent liquid.

[0098] Example 6 (Preparation of thermosetting resin, mainly used as a binder for refractory materials such as three large parts)

[0099] Add 63 parts of the dehydrated and layered o-para-phenol mixture of the previous batch into a reactor, add 400 parts of 99.83% high-purity o-meta-para-phenol obtained in Example 1 [meta-cresol: (o-cresol + o-ethylphenol + p-cresol) is 32.4:67.6], 30 parts of 25% ammonia water, and 3 parts of ethanolamine (the amount of ammonia water and ethanolamine is 1.86% of the mass of o-para-phenol), stir evenly, turn off the steam when the temperature is about 70-75°C, slowly raise the temperature to 90-95°C, turn on the cooling water, and drop 545 parts of 37% formaldehyde (the total molar ratio of formaldehyde to phenol is 1.30:1) for 4 hours. After the dropwise addition, add the remaining 100 parts of high-purity o-meta-para-phenol, and continue to keep warm for 2 hours.

[0100] After the reaction is completed, add glacial acetic acid to neutralize, maintain for 10 minutes, start the vacuum pump to evacuate, and start dehydration after the vacuum is stable. When the dehydration speed slows down or the temperature drops to about 70-75°C, turn on the steam heating. During dehydration, the steam switch should be continuously adjusted according to the speed of water output to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at about 90°C. When the water level reaches the required value (447 parts, the actual value is subject to production data), samples are taken to analyze the moisture and viscosity. When the moisture is 2-3%, stop evacuation, and add ethylene glycol to adjust the viscosity to the specified value of 15-20Pa.s. After the viscosity reaches the requirement, cool down to 50°C and discharge 699 parts of the material. The material is a yellow to light red transparent liquid.

[0101] The separated water was allowed to stand for 1 hour to separate into layers, and 63 parts of an o-para-phenol mixture (o-cresol / p-cresol / o-ethylphenol mixture) were obtained for application. The separated water layer was sent to the three waste workshop for treatment.

[0102] Example 7 (Preparation of thermosetting resin, electronic material)

[0103] Add 108 parts of the crude o-cresol mixture of the dehydrated layers in the previous batch into a reactor, add 250 parts of the o-cresol enriched fraction obtained in Example 1 (25.5% phenol, 74.4% o-cresol), 30 parts of 25% ammonia water, and 3 parts of ethanolamine (the amount of ammonia water and ethanolamine is 1.73% of the mass of o-para-phenol), stir evenly, heat to about 70-75°C, turn off the steam, slowly heat to 90-95°C, turn on the cooling water, and drop 545 parts of 37% formaldehyde (the total molar ratio of formaldehyde to phenol is 1.16:1) for 4 hours. After the dropwise addition, add the remaining 250 parts of the o-cresol enriched fraction, and continue to keep warm for 3 hours.

[0104] After the reaction is completed, add glacial acetic acid for neutralization, maintain for 10 minutes, start the vacuum pump to evacuate, and start dehydration after the vacuum is stable. When the dehydration speed slows down or the temperature drops to about 70-75°C, turn on the steam heating. During dehydration, the steam switch should be continuously adjusted according to the speed of water output to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at about 90°C. When the water level reaches the required value (461 parts, the actual value is subject to production data), samples are taken for analysis of moisture and viscosity. When the moisture is 2-3%, stop evacuation, and add ethylene glycol to adjust the viscosity to the specified value of 15-20Pa.s. After the viscosity reaches the requirement, cool down to 50°C and discharge 691 parts of the material. The material is a yellow to light red transparent liquid.

[0105] The separated water was allowed to stand for 1 hour to separate into layers, and 108 parts of crude o-cresol were obtained (content 98.6%, which can also be distilled to obtain 99.5% petrochemical o-cresol). The separated water layer was sent to the three waste workshop for treatment.

[0106] Example 8 (Preparation of thermosetting resin, thermal insulation material, refractory material, etc.)

[0107] Add 102 parts of the o-cresol / p-cresol / o-ethylphenol mixture dehydrated from the previous batch into a reactor, add 350 parts of 99.87% high-purity o-m-cresol in Example 2 [m-cresol: (o-ethylphenol + p-cresol + o-cresol) is 46.9:53.1], 7.5 parts of sodium carbonate (dissolved in 20 parts of water) (the amount of sodium carbonate is 1.25% of the total mass of phenol), stir evenly, turn off the steam when the temperature is about 65-70°C, slowly raise the temperature to 80-85°C, turn on the cooling water, and drop 545 parts of 37% formaldehyde (the total molar ratio of formaldehyde to phenol is 1.24:1), the dropwise addition time is 4 hours, add the remaining 150 parts of high-purity o-m-cresol within 1 hour after the dropwise addition is completed, and react at 80-85°C for 2 hours.

[0108] After the reaction is completed, 7 parts of glacial acetic acid and 0.1 parts of 85% phosphoric acid are added for neutralization, and the vacuum pump is started for 10 minutes to evacuate the mixture. After the vacuum is stable, dehydration is started. When the dehydration speed slows down or the temperature drops to about 70-75°C, steam heating is turned on. During dehydration, the steam switch should be continuously adjusted according to the speed of water discharge to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at about 100°C. When the water level reaches the required value (about 480 parts, the actual value is subject to production data), samples are taken for analysis of moisture and viscosity. When the moisture is 2-3%, vacuuming is stopped, and ethanol is added to adjust the viscosity to the specified value of 15-20 Pa.s. After the viscosity reaches the requirement, the temperature is lowered to 50°C and 698 parts of material are discharged.

[0109] The separated water was allowed to stand for 1 hour to separate into layers, and 102 parts of a mixture of o-cresol / p-cresol / o-ethylphenol were obtained for application. The separated water layer was sent to the three waste workshop for treatment.

[0110] Comparative Example 1 (Preparation of Thermosetting Resin)

[0111] Add 500 parts of petrochemical-grade 99.9% phenol, 5 parts of flake caustic soda (dissolved in 10 parts of water) (the amount of flake caustic soda is 1% of the total mass of phenol), and 545 parts of formaldehyde in the reactor in sequence (the total molar ratio of formaldehyde to phenol is 1.26:1). Raise the temperature to around 40-45°C, turn off the steam, turn on the cooling water at 50-55°C, slowly raise the temperature to 80-85°C, and keep the reaction for 2 hours. Pay more attention to the temperature changes of the materials before and after turning on and off the steam and cooling water.

[0112] After the reaction is completed, add glacial acetic acid for neutralization, maintain for 10 minutes, start the vacuum pump to evacuate, and start dehydration after the vacuum is stable. When the dehydration speed slows down or the temperature drops to about 70-75°C, turn on the steam heating. During dehydration, the steam switch should be continuously adjusted according to the speed of water output to complete the dehydration at a lower temperature as much as possible. In the later stage, steam can be continuously passed to control the final temperature of the liquid at about 80°C. When the water level reaches the required value (413 parts, the actual value is subject to production data), samples are taken for analysis of moisture and viscosity. When the moisture is 2-3%, stop evacuation, and add ethylene glycol to adjust the viscosity to the specified value of 10-15 Pa.s. After the viscosity reaches the requirement, cool down to 50°C and discharge 688 parts.

[0113] The thermosetting phenolic resins prepared in Examples 5-8 and Comparative Example 1 were tested and compared in terms of solid content, residual carbon rate, free phenol, free aldehyde, etc. The results are shown in Table 5:

[0114] Table 5

[0115]

[0116] It can be seen from Table 5 that the thermosetting phenolic resins synthesized from mixed phenols and high-purity o-meta-para-phenol in Examples 4, 5, 6 and 7 are consistent with the resin data synthesized from petrochemical phenol in terms of main indicators such as solid content, residual carbon rate, free phenol and free aldehyde, and the solid content and residual carbon rate are higher than those in Comparative Example 1.

[0117] Example 9 (Preparation of thermoplastic resin)

[0118] Liquid resin production:

[0119] Start stirring in the reactor, add 350 parts of the phenol / o-cresol fraction obtained in Example 3 (86% phenol, 13.9% o-cresol), 4 parts of oxalic acid (dissolved in 8 parts of water) (the amount of oxalic acid is 0.8% of the total mass of phenol), and 210 parts of formaldehyde in one feed (the total molar ratio of formaldehyde to phenol is 0.73:1).

[0120] After the feeding is completed, use pH test paper to determine the pH of the reaction liquid to be 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate should be strictly controlled within 1-3℃ / min to avoid heating too quickly, which will cause the reaction liquid to leak out and affect the resin quality.

[0121] Heat to 95°C, start heat preservation reaction, control the reaction temperature at 95-100°C, heat preservation reaction for 1 hour, then add the remaining 100 parts of 37% formaldehyde and 150 parts of phenol / o-cresol fractions within 1 hour, and finish heat preservation reaction. Pay close attention to the whitening time during the reaction, add 2 parts of 36% hydrochloric acid (36% hydrochloric acid is 0.4% of the total mass of phenol) after 0.5 hours of whitening, continue heat preservation reaction for 1 hour, and after judging the reaction end point, add 2.5 parts of caustic soda (5 parts water-soluble) for neutralization.

[0122] When the pH value of the neutralization reaction liquid is determined to be 6.0-7.0 by test paper, adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally at 252 parts. The specific water level shall be constant within 20 minutes.

[0123] After confirming that dehydration is complete, add ethylene glycol to dilute. When the resin temperature drops to 78°C, add ethanol to dilute. After stirring for 0.5 hour, measure the viscosity. Finally, adjust to the required viscosity with the specified ratio of ethylene glycol to ethanol. After the viscosity is adjusted, stir for another hour, cool naturally, and discharge the material when the resin temperature is less than 70°C to obtain 551 parts.

[0124] Example 10 (Preparation of thermoplastic resin)

[0125] Production of solid resins:

[0126] Stirring was started in the reactor, and 400 parts of the o-cresol enriched fraction obtained in Example 3 (19.06% phenol, 80.86% o-cresol), 8 parts of oxalic acid (dissolved in 8 parts of water) (the total amount of oxalic acid was 2.4% of the total mass of phenol), and 210 parts of formaldehyde were added at once. (The total molar ratio of formaldehyde to phenol was 0.80:1)

[0127] After the feeding is completed, use pH test paper to determine the pH of the reaction liquid to be 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate should be strictly controlled within 1-3℃ / min to avoid heating too quickly, which will cause the reaction liquid to leak out and affect the resin quality.

[0128] The temperature was raised to 95°C, and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C. After the heat preservation reaction for 1 hour, the remaining 100 parts of 37% formaldehyde and 100 parts of o-cresol enriched fraction were added dropwise within 1 hour, and the heat preservation reaction was completed. During the reaction, the whitening time should be paid close attention. After the whitening time was 0.5 hours, 4 parts of oxalic acid were added, and the heat preservation reaction was continued for 2 hours. The reaction was terminated after the reaction endpoint was determined.

[0129] Adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally at 235 parts, and the specific water level is based on whether it is constant within 20 minutes; then gradually increase the vacuum degree to -0.09-0.095Mpa, distill to a liquid temperature of 150°C in about 1-2 hours, discharge the material while hot into a stainless steel plate, cool it, and then break it to obtain 471 parts of light yellow to yellow small pieces of transparent solid.

[0130] The water layer was distilled to obtain 89 parts of crude o-cresol (content 98.3%), and the water layer was sent to the three wastes treatment section.

[0131] Example 11 (Preparation of thermoplastic resin)

[0132] Liquid resin production:

[0133] Start stirring in the reactor, add 400 parts of 99.83% high-purity o-para-cresol obtained in Example 1 [m-cresol: (o-cresol + o-ethylphenol + p-cresol) is 32.4:67.6], 4 parts of oxalic acid (dissolved in 8 parts of water) (the total amount of oxalic acid is 0.8% of the total mass of phenol), and 210 parts of formaldehyde (the total molar ratio of formaldehyde to phenol is 0.84:1) at one time.

[0134] After the feeding is completed, use pH test paper to determine the pH of the reaction liquid to be 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate is strictly controlled within 1-3℃ / min. The rate is determined to be 1.5-2℃ / min to avoid heating too fast, which will cause the reaction liquid to bubble out and affect the resin quality.

[0135] The temperature was raised to 95°C and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C and stabilized at 98°C. After the heat preservation reaction for 1 hour, the remaining 100 parts of 37% formaldehyde and 100 parts of high-purity o-para-phenol were added dropwise within another 1 hour to complete the heat preservation reaction.

[0136] Pay close attention to the whitening time during the reaction process. Add 2 parts of 36% hydrochloric acid (the amount of 36% hydrochloric acid is 0.4% of the total mass of phenol) after whitening for 0.5 hour, continue to keep warm and react for 1 hour. After judging the reaction endpoint, add 2.5 parts of caustic soda (5 parts water-soluble) to neutralize to pH 6-7.

[0137] When the pH value of the neutralization reaction liquid is determined to be 6.0-7.0 by test paper, adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally at 229 parts. The specific water level shall be constant within 20 minutes.

[0138] After confirming that the dehydration is complete, release half of the material into another kettle and dilute it with ethylene glycol. When the resin temperature drops to 78°C, add ethanol to dilute it. After stirring for 0.5 hours, measure the viscosity initially. Finally, adjust to the required viscosity with the specified ratio of ethylene glycol to ethanol.

[0139] After the viscosity is adjusted, stir for another hour, cool naturally, and discharge the material when the resin temperature is less than 70°C to obtain 560 parts.

[0140] Example 12 (Preparation of thermoplastic resin)

[0141] Production of solid resins:

[0142] Start stirring in the reactor, add 500 parts of 99.83% high-purity o-meta-para-phenol obtained in Example 1 [m-cresol: (o-cresol + o-ethylphenol + p-cresol) is 32.4:67.6], 70 parts of o-cresol / p-cresol / o-ethylphenol recovered from the water layer, 4 parts of oxalic acid (dissolved in 8 parts of water) (the total amount of oxalic acid is 0.7% of the total mass of phenol), and 240 parts of formaldehyde (the total molar ratio of formaldehyde to phenol is 0.84:1) at one time.

[0143] After the feeding is completed, use pH test paper to determine the pH of the reaction liquid to be 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate should be strictly controlled within 1-3℃ / min to avoid heating too quickly, which will cause the reaction liquid to leak out and affect the resin quality.

[0144] The temperature was raised to 95°C and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C. After the heat preservation reaction for 1 hour, the remaining 115 parts of 37% formaldehyde were added dropwise within 1 hour to complete the heat preservation reaction. During the reaction, the whitening time should be paid close attention. After the whitening for 0.5 hours, 2 parts of 36% hydrochloric acid (the amount of 36% hydrochloric acid is 0.4% of the total mass of phenol) were added. The heat preservation reaction was continued for 1 hour. The reaction was terminated after the reaction endpoint was determined.

[0145] Adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally at 265 parts, and the specific water level is constant within 20 minutes. Then gradually increase the vacuum degree to -0.09-0.095Mpa, distill to a liquid temperature of 130°C in 2 hours, discharge the material while hot into a stainless steel plate, cool it, and then break it to obtain 559 parts of light yellow to yellow small pieces of transparent solid.

[0146] The distilled water layer obtained 71.2 parts of o-cresol / p-cresol / o-ethylphenol (o-para content 98.7%), and the water layer was sent to the three wastes treatment section.

[0147] Example 13 (Preparation of m-cresol-formaldehyde resin for photoresist)

[0148] In the reaction kettle, 500 parts of high-purity o-para-o-cresol (containing 0.12% o-cresol, 37.77% p-cresol, 61.06% m-cresol, 0.09% 2,6-xylenol, 0.79% o-ethylphenol, and 0.0.09% 2,4 / 2,5-xylenol) extracted from Example 4, 2.4 parts of oxalic acid (4 parts dissolved in hot water), and 1.2 kg of formic acid (the amount of catalyst is 0.72% of the total mass of phenol) were added; after the feeding was completed, the steam valve was opened to increase the temperature, and the steam pressure should not exceed 0.3 MPa. 79.2 parts of paraformaldehyde (phenol: aldehyde molar ratio is 1:0.54) were gradually added to the kettle at 80°C for 2 hours, and the temperature was slowly increased after the addition; the heating rate was strictly controlled within 1-3°C / min, and the rate was determined to be 1.5-2°C / min to avoid excessive heating and causing the reaction solution to bubble out.

[0149] The temperature was raised to 95°C and the heat preservation reaction was started. The reaction temperature was controlled at 95-100°C. The temperature was kept for 2 hours and samples were taken for analysis. Liquid chromatography analysis showed that 0.15% of m-cresol was qualified.

[0150] The temperature was raised for distillation, and the evaporated gas was condensed in the reflux condenser and entered the water separator, and the upper layer was water, which was refluxed into the reactor for application, and the lower layer was o-cresol / p-cresol / o-ethylphenol mixed phenol, which was collected in a collection tank. After there was no obvious oil in the evaporated condensate, 9.6 parts of a solution containing recovered piperidine acetate catalyst and 0.3 parts of piperidine acetate adduct were added to the reactor material and mixed, and the vacuum device was adjusted to start vacuum dehydration. The dehydration temperature was controlled at 80-85°C, the time was controlled at 2-3 hours, and the final pressure was controlled at -0.075-0.08Mpa. At the same time, the water level of the receiver was observed, and the specific water level was constant within 20 minutes. The above collected water layers obtained 162 parts of a crude p-cresol mixture (p-cresol content 98.11%, o-ethylphenol 1.83%).

[0151] The vacuum degree was gradually increased to 0.098MPa, and the temperature was further increased for dehydration. When the temperature of the material in the kettle reached 190°C and no liquid was distilled out, the temperature was kept for 1 hour, the dehydration was stopped, and the vacuum was released with nitrogen. The material was placed in a stainless steel plate while hot under the protection of nitrogen, cooled, and then crushed and bagged to obtain 374.8 parts of m-cresol-formaldehyde resin, which was off-white to light yellow in color. The 9.6 parts of the solution containing the piperidine acetate catalyst collected in this step were used. The sample was taken for gel chromatography to determine the molecular weight (Mw 10386) and the dispersion was 2.35; at the same time, the experimentally measured resolution was 0.33μm.

[0152] Preparation of piperidine acetate adduct: piperidine is added dropwise to glacial acetic acid under stirring at a weight ratio of piperidine / glacial acetic acid = 1 / 2, and the temperature is controlled below 50°C. After mixing, the mixed solvent is recovered under reduced pressure until it is almost dry. The distilled mixed solvent is set aside for use. (Physical parameters of the mixed solvent: boiling point 165-170°C).

[0153] Comparative Example 2 (thermoplastic resin, refractory material, thermal insulation material, etc.)

[0154] Start stirring, add 500 parts of phenol, 3.5 parts of oxalic acid (7 parts dissolved), and 347 parts of formaldehyde into the reactor; after the feeding is completed, use pH paper to determine that the pH of the reaction liquid is 1-2, adjust the reflux and venting devices, open the steam valve to increase the temperature, the steam pressure should not exceed 0.5Mpa, and the heating rate is strictly controlled within 2℃ / min, and the rate is determined to be 1.5℃ / min to avoid heating too fast, which will cause the reaction liquid to bubble out and affect the resin quality.

[0155] Heat to 95°C and start heat preservation reaction. The reaction temperature is controlled at 95-100°C and stabilized at 98°C. Pay close attention to the whitening time during the reaction. Add 1.9 parts of hydrochloric acid after whitening for 0.5 hour, continue to keep warm for 1 hour, and after judging the reaction endpoint, add 2.5 parts of flake caustic soda (5 parts water dissolved) for neutralization.

[0156] When the pH value of the neutralization reaction liquid is determined to be 6.0-7.0 by test paper, adjust the vacuum device and start vacuum dehydration. The dehydration temperature is controlled at 80-85°C and the final pressure is controlled at -0.075-0.08Mpa. At the same time, observe the water level of the receiver. The water level is generally between 235 and 265 parts. The specific water level shall be constant within 20 minutes.

[0157] After confirming that dehydration is complete, add 40 parts of ethylene glycol for dilution. When the resin temperature drops to 78°C, add ethanol to dilute and adjust to 10-15 Pa.s. After the viscosity is adjusted, stir for another hour, cool naturally, and discharge 546 parts of the material when the resin temperature is less than 70°C.

[0158] Table 6

[0159]

[0160] It can be seen from Table 6 that the thermosetting phenolic resins synthesized from mixed phenols and high-purity o-para-phenol in Examples 9, 10 and 11 are consistent with the data of the resin synthesized from petrochemical phenol in terms of major indicators such as moisture content, solid content, residual carbon rate, and free phenol. The solid content and residual carbon rate of the thermoplastic phenolic resin synthesized from high-purity o-para-cresol are higher than those in Comparative Example 2.

[0161] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for extracting high-purity o-para-phenol from mixed cresols, characterized in that: Adding mixed cresols to a stirred reactor, sampling and analyzing the contents of aniline and organic acid in the mixed cresols, adding reagents for treatment according to the analysis results, and then adding the treated mixed cresols to the reactor of a high-efficiency distillation tower, after reflux dehydration, adding 0.01-1% concentrated sulfuric acid of the mass of the mixed cresols to continue oxidation and impurity removal, and at the same time, performing vacuum distillation at the top of the tower to obtain high-purity o-meta-para-phenol with a content of 99%; The high-purity o-para-p-phenol with a content of 99% is used as a raw material for synthesizing m-cresol-formaldehyde resin; The mixed cresols are derived from crude phenol from coal gasification, crude phenol from coking, crude phenol in water or crude phenol extracted from gasified and pyrolyzed coal tar.

2. The method for extracting high-purity o-para-phenol from mixed cresols as claimed in claim 1, characterized in that: The method of adding reagents for treatment according to the analysis results is as follows: if the content of organic acid in the mixed cresol is higher than that of aniline, the reagent added is 1 to 1.5 times the molar amount of sodium bicarbonate of the organic acid; if the content of aniline in the mixed cresol is higher than that of organic acid, the reagent added is 1 to 1.5 times the molar amount of sulfuric acid of the aniline; if the molar amount of aniline to organic acid is (0.95 to 1.05):1, the reagent added is 0.5 to 1.0 times the molar amount of sulfuric acid of the aniline.

3. The method for extracting high-purity o-para-phenol from mixed cresols as claimed in claim 1, characterized in that: The number of theoretical plates of the high-efficiency distillation tower is 200-350.

4. The method for extracting high-purity o-para-phenol from mixed cresols as claimed in claim 1, characterized in that: The reflux ratio of the vacuum distillation is (5-30):1, and the pressure of the vacuum distillation is -0.05--0.1Mpa.

5. The method for extracting high-purity o-para-phenol from mixed cresols as claimed in claim 4, characterized in that: The reflux ratio of the distillation is (15-20):

1.

6. The method for extracting high-purity o-para-phenol from mixed cresols according to any one of claims 1 to 5, characterized in that: When the mixed cresols are derived from crude phenol from coal gasification, crude phenol from coking or crude phenol from water, after vacuum distillation, in addition to obtaining high-purity o- and m-para-phenols with a content of 99%, the following fractions are also obtained: 95% phenol, a mixed phenol fraction with o-cresol ≤ 20%, a mixed phenol fraction with an o-cresol content of 20% to 50%, an o-cresol-enriched fraction, 99.5% o-cresol, and an o-cresol post-fraction containing 2,6-dimethylphenol; wherein 95% phenol, o-cresol ≤ 2 The mixed phenol fraction with 0% content and the mixed phenol fraction with 20% to 50% content of o-cresol are used to produce phenolic resin; the o-cresol enriched fraction is re-distilled to prepare 99.5% o-cresol; 99.5% o-cresol is used to produce o-cresol epoxy phenolic resin for electronic plastic packaging and pesticide 2-methyl-4-chlorophenol; the o-cresol post-fraction containing 2,6-dimethylphenol is used to produce 35% cresol for wire enamel, or to produce o-methyl anisole and 2,6-dimethyl anisole; When the mixed cresols are derived from crude phenol extracted from gasified and pyrolyzed coal tar, after vacuum distillation, in addition to obtaining high-purity o-meta-paraphenol with a content of 99%, the following fractions are also obtained: a phenol / o-cresol fraction with an o-cresol content of ≤20%, a mixed phenol fraction with an o-cresol content of 20% to 50%, an o-cresol-enriched fraction, 99.5% o-cresol, an o-cresol / 2,6-xylenol fraction, and a crude 2,4 / 2,5-xylenol product; Among them, the phenol / o-cresol fraction with o-cresol ≤ 20% and the mixed phenol fraction with o-cresol content of 20% to 50% are used to produce phenolic resin; the o-cresol enriched fraction is re-distilled to prepare 99.5% o-cresol; the o-cresol / 2,6-xylenol fraction is used to separate and produce pure 2,6-xylenol; the crude 2,4 / 2,5-xylenol is used to separate and produce 6-tert-butyl-2,4-xylenol and 99% 2,5-xylenol.

7. A method for synthesizing m-cresol-formaldehyde resin for photoresist using the high-purity o-m-para-phenol obtained by the method according to any one of claims 1 to 6, comprising the following steps: (1) adding high-purity ortho-para-phenol and an acidic catalyst into a reaction kettle, heating to 80° C., adding paraformaldehyde or formaldehyde in batches, heating to 95° C. to 100° C. at a heating rate of 1 to 3° C. / min after the addition, keeping the temperature for reaction for 2 to 4 hours, sampling and analyzing the cresol content in the reaction solution, and determining the content of cresols ≤ 0.5% as qualified. If the content is unqualified, adding a small amount of paraformaldehyde or formaldehyde and continuing the reaction until the content is qualified; (2) heating the reaction liquid to perform steam distillation, condensing the evaporated gas in a reflux condenser and entering a water separator, and separating the layers in the water separator, wherein the upper layer is water and is refluxed into the reaction kettle for application, and the lower layer is a mixed phenol of o-cresol / p-cresol / o-ethylphenol and is collected in a collection tank. After no obvious oily substance is found in the evaporated condensate, piperidine acetate adduct is added to the reaction liquid and mixed, and the vacuum device is adjusted to start vacuum dehydration, the dehydration temperature is 80 to 85° C., the time is 2 to 3 hours, and the final pressure is controlled to be -0.075 to -0.08 MPa. At the same time, the water level of the receiver is observed, and the collected water and the o-cresol / p-cresol / o-ethylphenol mixture are respectively combined when the water level is constant within 20 minutes; (3) gradually increasing the vacuum degree to 0.098 MPa, further increasing the temperature for dehydration, and when the temperature of the material in the kettle reaches 190° C. and no liquid is distilled out, keeping the temperature for 1 hour, stopping the dehydration, and removing the vacuum with nitrogen. Under the protection of nitrogen, discharge the material while hot into a stainless steel plate, and after cooling, break it into pieces and bag it to obtain m-cresol-formaldehyde resin; In step (2), the preparation method of the piperidine acetate adduct is as follows: piperidine is added dropwise to glacial acetic acid in a mass ratio of 4:(5-11), the temperature is controlled to be lower than 50° C., and after mixing, the mixed solvent is recovered under reduced pressure to obtain the product.

8. The method for synthesizing m-cresol-formaldehyde resin for photoresist as claimed in claim 7, characterized in that: In step (1), the acidic catalyst is a mixture of oxalic acid and formic acid in a molar ratio of (2-8):(0.1-1), and the amount used is 0.5-5% of the mass of high-purity o-meta-para-phenol.

Citation Information

Patent Citations

  • Method for preparing phenolic resin used for wire enamel

    CN101602837A

  • Method for preparing dephenolized oil and phenolic resin through medium and low temperature coal tar oil

    CN103289718A

  • Device and process for preparing phenolic resin from coal tar

    CN106543389A

  • Phenolic resin for photoresist and preparation method thereof

    CN113773460A

  • Phenolic resin and photoresist

    CN115850623A

Cited By

  • Method for synthesizing high-carbon phenolic resin and extracting ortho-position and para-position alkylphenol

    CN122037099A