Yellow copper halide fluorescent material as well as preparation method and application thereof

By developing yellow copper halide fluorescent material (pmib)4Cu4I4, the problem of low photochemical stability of existing materials under ultraviolet irradiation is solved, and good thermal stability and color stability are achieved at high temperatures. It is suitable for full-spectrum white LEDs, which is significantly Improved optical performance.

CN119060072AInactive Publication Date: 2024-12-03CHANGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410575582.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing yellow fluorescent materials have low photochemical stability under ultraviolet irradiation and exhibit poor absorption bands in visible light areas, making it difficult to replace rare earth phosphors as efficient yellow phosphors.

Method used

A yellow copper halide fluorescent material has been developed, with a single crystal structure of (pmib)4Cu4I4. It forms a classic [Cu4I4] tetrahedral coordination mode through Cu+ quadcoordination, and connects Cu atoms to ligand pmib to form a three-dimensional pore structure. , exhibiting emission and high thermal stability close to pure white.

Benefits of technology

The material exhibits good thermal stability and color stability at high temperatures, has a high color rendering index, and is suitable for full-spectrum white LEDs, which significantly improves optical performance and application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060072A_ABST
    Figure CN119060072A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of crystalline functional materials, and particularly relates to a yellow copper halide fluorescent material as well as a preparation method and application thereof, the molecular formula of a single crystal structure of the fluorescent material is (pmib) 4Cu4I4, and pmib is 1, 4-bis (imidazole-1-yl methyl) benzene. According to the invention, a copper halide coordination polymer is combined with a 365 nm-emitting ultraviolet chip to prepare a white LED (pc-wLED) converted by fluorescent powder, and the white LED shows remarkable optical properties under the working current of 100 mA: CCT (Coordinate of Cathode) = 4741 K, Ra = 85.9, and CIE (Coordinate of International Electronics) (0.3467, 0.3125). In addition, under excitation of 365nm ultraviolet light, the complex fluorescent powder shows emission close to pure white, and has a relatively high color rendering index.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of crystalline functional materials, and particularly relates to a yellow copper halide fluorescent material and a preparation method and application thereof. Background Art

[0002] Light-emitting diodes (LEDs) have been widely used as the next generation of light sources due to their high efficiency, long operating life, and high reliability. White LEDs (w-LEDs) with high color rendering index (CRI) and low correlated color temperature (CCT) in indoor lighting can usually be obtained by using blue-emitting LED chips to excite yellow phosphors. For example, blue InGaN LED chips (440-480nm) and yellow Y3Al5O 12 :Ce 3+ (YAG:Ce 3+ ) phosphors are commonly used to manufacture commercial w-LEDs. Considering the sustainable development and environmental protection of LED technology, it is very necessary to develop cheap metal complexes as efficient yellow phosphors to replace rare earth w-LEDs.

[0003] In recent years, copper halide complexes have been widely studied as promising fluorescent agents due to their wide excitation band, tunable emission band and high quantum yield in the ultraviolet region. Among them, metal halides with the molecular formula [M4X4L4] (M = Cu; X = Cl, Br or I; L = N- or P-terminal ligand) are excellent molecular fluorescent agents. However, such complexes often have shortcomings such as low photochemical stability under ultraviolet irradiation conditions and generally exhibit poor absorption bands in the visible light region. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a yellow copper halide fluorescent material. The single crystal structure formula of the fluorescent material is (pmib)4Cu4I4, wherein pmib is 1,4-bis(imidazol-1-ylmethyl)benzene, which is an imidazole ligand with an extended molecular structure. + It is four-coordinated. The smallest asymmetric unit structure center of the complex is composed of four crystallographically independent Cu and four I atoms, forming a classic [Cu4I4] tetrahedral coordination mode, and then the Cu atom and the ligand pmib are connected to form a three-dimensional channel structure.

[0005] The complex fluorescent material shows nearly pure white emission under the excitation of light waves of corresponding wavelengths, has a high color rendering index, and has good thermal stability and color stability at high temperatures.

[0006] The present invention also provides a method for preparing the yellow copper halide fluorescent material.

[0007] (1) Preparation of organic ligand PMIB

[0008] In an alkaline dry environment, 2-methylimidazole reacts with α-α'-dichloro-p-xylene to generate 1,1'-[1,4-phenylenebis(methylene)]bis[2-methyl-1H-imidazole] (organic ligand pmib):

[0009]

[0010] Specifically:

[0011] After 2-methylimidazole and potassium hydroxide are fully mixed in dimethyl sulfoxide, α-α'-dichloro-p-xylene in a molar ratio of 4.9-5.1:9.9-10.2 to 2-methylimidazole is added thereto, and the reaction is fully stirred, and liquid-liquid extraction is performed with dichloromethane and then separated. The separated organic phase containing the product is washed with water, and then anhydrous magnesium sulfate is added thereto to absorb water, and then the magnesium sulfate is filtered out, and the obtained filtrate is concentrated and ether is added thereto, and after the precipitate is fully precipitated at low temperature, the precipitate is collected as an organic ligand pmib product, and the product is a yellow powder.

[0012] Among them, potassium hydroxide, as a catalyst, does not participate in the reaction and can improve the efficiency of the reaction;

[0013] (2) Organic complex [(pmib)4Cu4I4] n Preparation

[0014] The organic ligand pmib and CuI obtained in step (1) are mixed with acetonitrile and water in a molar ratio of 0.09-0.11:0.36-0.44, and then heated to react fully. After natural cooling, the mixture is filtered. The filter cake is washed fully and then dried to obtain an organic complex [(pmib)4Cu4I4] n , as pure bright yellow crystals:

[0015]

[0016] Preferably, in step (1), the molar ratio of potassium hydroxide to 2-methylimidazole is 40.8-41:9.9-10.2.

[0017] Preferably, in step (1), 2-methylimidazole and potassium hydroxide are stirred and mixed in dimethyl sulfoxide at room temperature (25° C., the same below) for 1.5 h to 2 h.

[0018] Preferably, in step (1), 2-methylimidazole and potassium hydroxide are fully mixed in dimethyl sulfoxide, α-α'-dichloroparaxylene is added thereto, and the mixture is stirred and reacted at room temperature for 10 to 12 hours.

[0019] Preferably, in step (2), the volume ratio of acetonitrile to water is 5.9-6.1:1.9-2.1.

[0020] Preferably, in step (2), the organic ligand pmib and CuI obtained in step (1) are mixed with acetonitrile and water in a polytetrafluoroethylene autoclave, and then heated to 165° C. to 175° C. to react for 70 to 74 hours.

[0021] The present invention also provides an application of the yellow copper halide fluorescent material as an ultraviolet light excitable fluorescent body in a full-spectrum white light LED.

[0022] Preferably, the fluorescent material is combined with a 365nm emitting UV chip to assemble into a white LED (pc-wLED). Under the excitation of 365nm UV light, the fluorescent material shows an emission close to pure white and has a high color rendering index.

[0023] As a preferred embodiment: fluorescent material and blue powder (BaMgAl 10 O 17 :Eu 2+ ) and then assembled with a blue light-emitting diode (LED) to form a pc-wLED.

[0024] The beneficial effects of the present invention are:

[0025] X-ray diffraction data show that the complex [(pmib)4Cu4I4] of the present invention n Crystallizes in the monoclinic C 2 / c space group. In the complex structure, copper atoms coordinate with iodine atoms to form a cubane structure, and together with the ligands weave into a three-dimensional pore structure. The three-dimensional material has good conductivity and optical properties, which makes them have a wide range of application prospects in the fields of electronic devices, optoelectronic devices and sensors, such as for the preparation of efficient photoelectric conversion devices to achieve efficient use of solar energy;

[0026] The complex of the present invention [(pmib)4Cu4I4] n It exhibits efficient solid-state emission at room temperature: in the fluorescence emission spectrum, the fluorescence emission of the complex is the strongest at an excitation wavelength of 390nm; the complex exhibits a strong emission band centered at 600nm, with a half-peak width (FWHM) of about 130nm. At the same time, the emission center of the complex has a tendency to move with increasing temperature, and when the temperature increases from 80K to 500K, the emission center of the complex has a slight blue shift of about 35nm, which indicates that with the change of temperature, the complex exhibits a relatively stable fluorescence color; through the study of temperature-dependent emission spectra, it can also be found that the complex [(pmib)4Cu4I4] of the present invention has a relatively stable fluorescence color. nThe invention has good thermal stability and color stability at high temperature; in a liquid nitrogen atmosphere, the complex [(pmib)4Cu4I4] n When heated from 80K to 500K, the fluorescence intensity of the complex is hardly quenched as the temperature increases, reflecting zero thermal quenching in a large temperature range.

[0027] The complex of the present invention [(pmib)4Cu4I4] n As white fluorescent powder and commercial blue powder (BaMgAl 10 O 17 :Eu 2+ ) and then assembled with a blue light-emitting diode (LED) to form a pc-wLED. The assembled pc-wLED showed significant optical properties at a working current of 100mA: CCT = 4741K, Ra = 85.9, CIE coordinates (0.3467, 0.3125). n It is a promising UV-excitable phosphor with great potential for application in full-spectrum white light LEDs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n X-ray crystal structure of the smallest unit;

[0029] Figure 2 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n 3D mesh structure diagram;

[0030] Figure 3 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Powder X-ray diffraction pattern of

[0031] Figure 4 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Infrared spectrum of

[0032] Figure 5 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Thermogravimetric diagram of

[0033] Figure 6 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Fluorescence excitation and emission spectra at 298K;

[0034] Figure 7 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Three-dimensional temperature-dependent fluorescence spectrum of

[0035] Figure 8 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Temperature-dependent fluorescence emission intensity integral diagram;

[0036] Fig. 9 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Temperature-dependent CIE diagram;

[0037] Fig.10 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n EL spectrum of a white LED (pc-wLED) assembled in combination with a 365nm emitting UV chip at a flux operating current of 10-300mA;

[0038] Fig.11 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n The working CIE variation trend of the white LED (pc-wLED) assembled in combination with a 365nm emitting UV chip;

[0039] Fig.12 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n The operating current-dependent EL intensity diagram of the white LED (pc-wLED) assembled in combination with a 365nm emitting UV chip;

[0040] Fig.13 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Photoluminescence quantum efficiency curve measured at 298K;

[0041] Fig.14 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Fluorescence lifetime decay curve at room temperature;

[0042] Fig.15 This is a graph showing the photoluminescence quantum efficiency of the organic complex prepared in Comparative Example 1 measured at 298K. DETAILED DESCRIPTION

[0043] The details of the reagents used in the following experimental process are shown in Table 1. These reagents were used directly without further purification. The details of the preparation equipment and detection instruments used in the following experimental process are shown in Table 2:

[0044] Table 1

[0045]

[0046]

[0047] Table 2

[0048] instrument Instrument Model Instrument manufacturer Oven DHG-9030A Gongyi City Yuhua Fourier Transform Infrared Spectrometer IR-50 Thermo Fisher Scientific X-ray single crystal diffractometer APEX-IIDUO Bruker, Germany Digital NMR Spectrometer AVANCE III 400M Bruker, Germany X-ray powder diffractometer D / MAX2500 Japanese Neo-Confucianism Thermogravimetric Analyzer Labsys Evo STA Setaram, France Rotary evaporator IKA HB 10 IKA, Germany Constant temperature heating magnetic stirrer CL-2 Shanghai Leici Xinjing Fluorometer FS5 Edinburgh, UK

[0049] Example 1

[0050] (1) Preparation of organic ligand PMIB

[0051] 10 mmol of 2-methylimidazole and 41 mmol of potassium hydroxide were added to 20 mL of dimethyl sulfoxide, stirred and mixed at room temperature for 2 hours, and then 5 mmol of α-α'-dichloro-p-xylene was added thereto. After stirring and reacting at room temperature for 12 hours, 50 mL of dichloromethane was used for liquid-liquid extraction and separation. The organic phase containing the separated product was washed with water, and then anhydrous magnesium sulfate was added thereto and stirred. After sufficient stirring, the magnesium sulfate was filtered out by suction, and the filtrate was retained. After the obtained filtrate was concentrated, an excess of ether was added thereto, and it was allowed to stand in a refrigerator at 2°C for 12 hours until the precipitate was fully precipitated, and the precipitate was collected as the organic ligand pmib product, and the product was a yellow powder;

[0052] (2) Organic complex [(pmib)4Cu4I4] n Preparation

[0053] 1 mmol of the organic ligand pmib obtained in step (1), 4 mmol of CuI, 6 mL of acetonitrile and 2 mL of water were sealed and mixed in a polytetrafluoroethylene autoclave with a volume of 15 mL, and reacted at 170°C for 72 hours. After naturally cooling to room temperature, the filter cake obtained by filtration was a bright yellow crystal suitable for X-ray diffraction analysis. The filter cake was washed repeatedly with distilled water and acetonitrile alternately, and then dried in air to obtain pure bright yellow crystals, which was the organic complex [(pmib)4Cu4I4] n (H NMR spectrum: δ (ppm) 2.20 (s, 6H), 5.11 (s, 4H), 6.75 (d, J = 1.17 Hz, 2H), 7.09 (d, J = 1.17 Hz, 2H), 7.12 (s, 4H)), the yield is 83% (calculated based on the molar amount of the added organic ligand pmib).

[0054] The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Elemental analysis: Theoretical value of elemental analysis (%) (C 16 H 18 Cu2I2N4): C 29.67; H 2.78; N 8.65, experimental value: C 29.69; H 2.76; N 8.83.

[0055] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The minimum unit structure of X-ray crystal is shown in the attached figure. Figure 1 shown.

[0056] The organic complex [(pmib)4Cu4I4] prepared in Example 1 n The three-dimensional network structure constructed by low-temperature SC-XRD data analysis is shown in the attached figure. Figure 2 As shown in the figure, the complex crystallizes in the monoclinic C2 / c space group. The center of the smallest asymmetric unit structure of the complex is composed of four crystallographically independent Cu and four I atoms, forming a classic [Cu4I4] tetrahedral coordination mode, and then expanding outward through the connection between Cu atoms and ligands pmib to form a three-dimensional channel structure, in which the Cu-Cu distance is less than It is smaller than the van der Waals radius of Cu atoms, indicating the existence of strong Cu····Cu interaction. [Cu4I4] is coordinated by three I atoms and one N atom, where the N atom comes from the ligand I atoms come from metal salts Therefore, the structure of the complex is that the coordination units of [Cu4I4] and the bridging ligand pmib are interconnected and arranged continuously to form a three-dimensional pore structure.

[0059] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The crystallographic data were obtained on the Iuker APEX-IICCD instrument with graphene monochromatic radiation. The data were collected under the Luker Instrument Service v4.2.2 and SAINT V8.34A packages for data collection, data reduction and unit optimization. The SHELXS package was used for the organic complex [(pmib)4Cu4I4] n The product structure was elucidated, and the crystal data were optimized using the full matrix least squares method using the SHELXL program package, and the absorption correction was performed using the multi-scan program package SADABS. The organic complex [(pmib)4Cu4I4]n The hydrogen atoms of the products were determined by the riding mode of the SHELXTL package. 2 Anisotropic optimization was performed on the surface of the nanostructured carbon nanotubes, and the organic complex [(pmib)4Cu4I4] was finally obtained. n The crystallographic data of the product are shown in Table 3. The organic complex [(pmib)4Cu4I4] n Partial bond length of the product The data of bond angle (°) are shown in Table 4:

[0060] Table 3: Organic complexes [(pmib)4Cu4I4] n Crystallographic parameters of

[0061]

[0062]

[0063] ( a R1=Σ(||F0|-|F c ||) / Σ|F0|; b wR2=[Σw(|F0 2 |-|F c 2 |) 2 / Σw|F0 2 | 2 ] 1 / 2 ; c GOF=[∑[w(F0 2 -F c 2 ) 2 ] / (N obs -N params )] 1 / 2 , based on the data I>2σ(I).)

[0064] Table 4: Organic complexes [(pmib)4Cu4I4] n Important bond lengths in the crystal structure of and bond angle (°)

[0065]

[0066]

[0067] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The powder X-ray diffraction pattern of Figure 3As shown in the figure, the dark chromatogram line at the bottom is drawn from experimental data, and the light chromatogram line at the top is obtained by computer simulation based on the crystal structure. It can be seen from the figure that the experimental value and the simulation value can be very consistent, indicating that the organic complex [(pmib)4Cu4I4] n It is pure phase.

[0068] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The infrared spectrum of Figure 4 Shown: IR (KBr pellet, cm -1 ):3452(s),3143(s).1575(s),1507(w),1399(s),1250(w),1137(m),1006(w),962(w),887(w),781(m),744(m),670(w), attached Figure 4 In the figure, the upper dark chromatogram is drawn from the data obtained by the ligand pmib, and the lower light chromatogram is drawn from the data of the organic complex [(pmib)4Cu4I4] n The obtained data are plotted, and it can be seen from the figure that the vibration contraction peaks of the ligand and the complex are almost the same, indicating the presence of corresponding organic ligands in the complex.

[0069] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The thermogravimetric diagram is shown in the attached Figure 5 As shown, attached Figure 5 The organic complex [(pmib)4Cu4I4] prepared in Example 1 n From the thermal stability at room temperature to 800 °C, it can be seen from the TGA curve that the complex exhibits good thermal stability, and its mass loss is divided into two steps: the first weight loss of the complex of about 27–30% was observed between 300 and 400 °C due to the removal of halogens and part of the ligands; the second weight loss between 400 and 800 °C can be attributed to the complete removal of the remaining ligands.

[0070] Example 1: Organic complex [(pmib)4Cu4I4] prepared n Fluorescence excitation and emission spectra at 298K (λ em =600nm) as attached Figure 6 As shown: the complex exhibits a strong emission band centered at 590nm, with a half-maximum width (FWHM) of about 130nm, and the fluorescence emission is strongest at an excitation wavelength of 390nm. At room temperature, the complex emits orange light with an emission center of 600nm. In addition, the complex exhibits excitation band coverage from deep ultraviolet light to blue light.

[0071] As shown in Table 5, the organic complex [(pmib)4Cu4I4] prepared in Example 1 n The photoluminescence quantum yield (PLQY) in the solid state is 57.53%, and the fluorescence decay rate (k r )(k r =Φ PL τ -1 ) is 6.21×10 4 s -1 , considering Φ PL =k r / (k r +k nr ), where k nr is the rate of the nonradiative process including nonradiative singlet decay and ISC, so the k of the complex nr The value is estimated to be 4.59×10 4 s -1 .

[0072] Table 5: Organic complexes [(pmib)4Cu4I4] n Solid-state photophysical data of the product at room temperature

[0073]

[0074] ( a Radiative rate constant calculated k r =Φ / τ. b Nonradiative rateconstant calculated k nr =(1-Φ) / τ.)

[0075] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The three-dimensional temperature-dependent fluorescence spectra are shown in the attached Figure 7 The temperature-dependent fluorescence emission intensity integral diagram is shown in the attached Figure 8 As shown, as the temperature gradually increases from 80K to 500K, the emission center of the complex exhibits a slight blue shift of about 35nm. The results show that the complex exhibits a relatively stable fluorescence color as the temperature changes.

[0076] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The temperature change CIE diagram is as follows Fig. 9As shown: With the increase of temperature, the luminescence of the complex changes from orange at low temperature (80K) to yellow at high temperature (500K). Correspondingly, the CIE coordinates change from (0.5824, 0.4106) at 80K to (0.4553, 0.4833) at 500K. The change of CIE coordinates is consistent with the fluorescence emission shift with increasing temperature.

[0077] The organic complex [(pmib)4Cu4I4] prepared in Example 1 n Combined with a 365nm emitting UV chip to assemble a white LED (pc-wLED), the EL spectrum at 10-300mA flux working current is shown in the attached figure. Fig.10 As shown in the attached Fig.11 The working current dependence EL intensity diagram is shown in the attached Fig.12 As shown:

[0078] As shown in Table 6, within the range of flux current (10-300 mA), CIE x (about 0.3509) and CIE y (about 0.3169) remain basically unchanged. When the flux current is 100 mA, based on the organic complex [(pmib)4Cu4I4] n The CRI value of the LED (pc-wLED) is as high as 85.9 and the CCT is 4741K. The low CCT and high CRI value show the good optical performance of pc-wLED at high flux current;

[0079] In addition, based on the yellow emitting organic complex [(pmib)4Cu4I4] n The electroluminescence (EL) intensity of the LED (pc-wLED) increases with the increase of current, and the electroluminescence spectrum covers the entire visible light region of 385-800nm ​​(i.e., white light emission), such as Fig.12 As shown, the electroluminescence intensity gradually increases in the range of 10-300 mA.

[0080] Table 6: Organic complexes [(pmib)4Cu4I4] n EL parameters of white LED (pc-wLED) at different currents

[0081]

[0082]

[0083] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The photoluminescence quantum efficiency curve measured at 298K is shown in the attached figure. Fig.13As shown, at 298K, the photoluminescence quantum yield (PLQY) of the solid complex is 57.53%.

[0084] Example 1: Organic complex [(pmib)4Cu4I4] prepared n The fluorescence lifetime decay curve at room temperature is shown in the attached figure. Fig.14 As shown, at 298K, the fluorescence lifetime of the complex is 9.26μs.

[0085] Comparative Example 1

[0086] The "α-α'-dichloro-p-xylene" in Example 1 is replaced with an equal mole of "α-α'-dichloro-o-xylene", and the other components and operations remain unchanged:

[0087] (1) Preparation of organic ligands

[0088] 10 mmol of 2-methylimidazole and 41 mmol of potassium hydroxide were dissolved in 20 mL of dimethyl sulfoxide and stirred at room temperature for 2 h, then 5 mmol of α-α'-dichloro-o-xylene was added thereto, and the mixture was stirred at room temperature for 12 h, and then liquid-liquid extraction was performed with 50 mL of dichloromethane and then separated. The organic phase containing the product was washed with water, and then anhydrous magnesium sulfate was added thereto and stirred. After sufficient stirring, the magnesium sulfate was filtered out by suction, and the filtrate was retained. After the filtrate was concentrated, an excess of ether was added thereto, and the mixture was allowed to stand in a refrigerator at 2°C for 12 h until the precipitate was fully precipitated, and the precipitate was collected as an organic ligand;

[0089] (2) Preparation of organic complexes

[0090] 1 mmol of the organic ligand obtained in step (1), 4 mmol of CuI, 6 mL of acetonitrile and 2 mL of water were sealed and mixed in a 15 mL polytetrafluoroethylene autoclave, and reacted at 170°C for 72 hours. After naturally cooling to room temperature, the filter cake was filtered, and the filter cake was washed repeatedly with distilled water and acetonitrile alternately and then dried in air.

[0091] The only difference between Comparative Example 1 and this solution is the relative position of the chloromethyl group in the ligand molecular structure. After the relative position of the chloromethyl group as a reactive group is changed from the para position in this solution to the ortho position in Comparative Example 1, the molecular crystal structure of the prepared assembled coordination polymer is only a one-dimensional long chain structure, and the long chains cannot be connected to each other, resulting in the coordination polymer prepared in Comparative Example 1 being unable to form the three-dimensional structure in this solution;

[0092] Refer to the attached Fig.13 The photoluminescence quantum efficiency curve of the organic complex prepared in Comparative Example 1 measured at 298K is shown in the attached figure. Fig.15As shown: at 298K, its photoluminescence quantum yield (PLQY) is only 14.47%.

Claims

1. A yellow copper halide fluorescent material, characterized in that: The single crystal structure molecular formula of the fluorescent material is (pmib)4Cu4I4, wherein the pmib is 1,4-bis(imidazol-1-ylmethyl)benzene.

2. The yellow copper halide fluorescent material according to claim 1, characterized in that: The fluorescent material is a monoclinic crystal with a space group of C 2 / c and crystal parameters of α=90°, β=90.118(2)°, γ=90°, Z=8, 3. A method for preparing a yellow copper halide fluorescent material, characterized in that: The preparation method is: (1) Preparation of organic ligand PMIB After 2-methylimidazole and potassium hydroxide are fully mixed in dimethyl sulfoxide, α-α'-dichloro-p-xylene in a molar ratio of 4.9-5.1:9.9-10.2 to the 2-methylimidazole is added thereto, and the mixture is stirred and reacted fully, and liquid-liquid extraction is performed with dichloromethane and then separated, and the separated organic phase containing the product is washed with water, and then anhydrous magnesium sulfate is added thereto, stirred and dried, and then the magnesium sulfate is filtered out, and the obtained filtrate is concentrated and ether is added thereto, and the mixture is placed at low temperature until the precipitate is fully precipitated, and the precipitate is collected as the organic ligand pmib; (2) Organic complex [(pmib)4Cu4I4] n Preparation The organic ligand pmib and CuI obtained in step (1) are mixed with acetonitrile and water in a molar ratio of 0.09-0.11:0.36-0.44, and then heated to fully react, and then naturally cooled and filtered. The obtained filter cake is fully washed and dried to obtain the organic complex [(pmib)4Cu4I4] n .

4. The method for preparing a yellow copper halide fluorescent material as claimed in claim 3, characterized in that: In step (1), the molar ratio of the potassium hydroxide to the 2-methylimidazole is 40.8-41:9.9-10.

2.

5. The method for preparing the yellow copper halide fluorescent material as claimed in claim 3, characterized in that: In step (1), the 2-methylimidazole and the potassium hydroxide are stirred and mixed in the dimethyl sulfoxide at room temperature for 1.5 hours to 2 hours.

6. The method for preparing the yellow copper halide fluorescent material as claimed in claim 3, characterized in that: In step (1), the 2-methylimidazole and the potassium hydroxide are fully mixed in the dimethyl sulfoxide, and then the α-α'-dichloroparaxylene is added thereto and stirred at room temperature for reaction for 10 h to 12 h.

7. The method for preparing the yellow copper halide fluorescent material as claimed in claim 3, characterized in that: In step (2), the volume ratio of the acetonitrile to the water is 5.9-6.1:1.9-2.

1.

8. The method for preparing the yellow copper halide fluorescent material as claimed in claim 3, characterized in that: In step (2), the organic ligand pmib obtained in step (1), the CuI, the acetonitrile and the water are mixed in a polytetrafluoroethylene high-pressure reactor, and then heated to 165° C. to 175° C. to react for 70 to 74 hours.

9. Use of the yellow copper halide fluorescent material as claimed in claim 1 or 2 as an ultraviolet light excitable phosphor in a full spectrum white light LED.

10. The use of the yellow copper halide fluorescent material as claimed in claim 9 as an ultraviolet light excitable fluorescent body in a full spectrum white light LED, characterized in that: The fluorescent material is combined with an ultraviolet chip emitting at 365 nm to assemble a white LED.

Citation Information

Patent Citations

  • Zero / negative heat quenching near-infrared photoluminescent material as well as preparation method and application thereof

    CN115246848A

  • Novel Cu (I) complex fluorescent material as well as preparation method and application thereof

    CN116554210A