A thermoassociated gel, its preparation method and application

By preparing a thermally associative gel formed by reacting alkenylamide monomers, functional monomers, and crosslinking agents, the problems of low structural strength and insufficient temperature resistance of existing gel-type plugging agents at high temperatures were solved, and the malignant leakage of the Tahe carbonate reservoir was effectively sealed.

CN119060248BActive Publication Date: 2026-11-17CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310648591.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2026-11-17
Estimated Expiration
2043-06-02

AI Technical Summary

Technical Problem

Existing gel-based plugging agents have low structural strength and limited temperature resistance under high-temperature conditions, and insufficient high-temperature stability. Furthermore, their formulations contain many components that are difficult to mix evenly, affecting their effectiveness in the field and making them unable to effectively seal the malignant leakage of the Tahe carbonate reservoir.

Method used

A thermoassociated gel was prepared by reacting alkenylamide monomers, functional monomers, and crosslinking agents under the action of an initiator, forming a plugging agent with high structural strength and good high-temperature resistance, which is suitable for the high-temperature and high-salinity Tahe carbonate reservoir.

Benefits of technology

At 140℃, the thermally associative gel has a structural strength of 3500Pa to 3750Pa, which can effectively seal cracks 1 to 3mm wide, and has a pressure resistance of 8MPa and can be maintained for at least 1 hour, achieving a long-term sealing effect and overcoming the shortcomings of existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060248B_ABST
    Figure CN119060248B_ABST
Patent Text Reader

Abstract

This invention provides a thermoassociated gel, its preparation method, and its application. The thermoassociated gel is obtained by reacting alkenylamide monomers, functional monomers, and a crosslinking agent under the action of an initiator, and possesses advantages such as high structural strength, good high-temperature resistance, and good plugging performance. The thermoassociated gel uses fewer raw materials, has a simple preparation method, and is a finished product before entering the formation. This overcomes the problems of existing technologies where the gel components are numerous, inconvenient to use, and difficult to mix evenly, thus affecting the plugging effect. It can be used as a plugging agent to continuously and effectively plug fractured-vuggy reservoirs at temperatures up to 140°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of reservoir plugging technology, and particularly relates to a thermally associative gel, its preparation method and application. Background Technology

[0002] The deep carbonate reservoirs in the Tarim Oilfield are characterized by well-developed fractures and cavities, exhibiting strong heterogeneity and making them highly susceptible to severe lost circulation during drilling. However, commonly used plugging agents such as bridging materials, cement, and high-fluidity-loss consolidation agents have poor applicability to fractured-cavity lost circulation in the Tarim Basin and cannot meet the drilling and plugging requirements for this type of reservoir. Compared with conventional plugging agents, gel plugging agents have advantages such as strong retention capacity and resistance to formation fluid dilution in fractured-cavity severe lost circulation. The research and application of this technology is of great significance for effectively sealing severe lost circulation in carbonate fractured-cavity reservoirs.

[0003] Existing gel-based sealants have the following main drawbacks when exposed to high-temperature environments:

[0004] (1) The gel main agent is mostly a polyacrylamide polymer, which has limited structural strength and temperature resistance;

[0005] (2) High temperatures will reduce the structural strength of the gel;

[0006] (3) The high temperature resistance time is too short, and it cannot continue to function at high temperatures, resulting in insufficient high temperature stability;

[0007] (4) The gel formulation has many components, making it inconvenient to use and difficult to mix evenly, which affects the on-site application effect.

[0008] The Tarim Basin carbonate reservoirs are characterized by high temperature and high salinity, specifically temperatures ranging from 120℃ to 140℃ and salinity from 210 g / L to 240 g / L. These characteristics, particularly the high temperature, limit the effective application of polyacrylamide polymer gel plugging agents in sealing leaks. Therefore, researching efficient plugging materials suitable for the Tarim Basin carbonate reservoirs is of paramount importance for the efficient drilling and development of deep Tarim Basin carbonate reservoirs, and this is a key issue that urgently needs to be addressed in this field. Summary of the Invention

[0009] To address the problems of low structural strength and limited temperature resistance of existing polymer gel sealing agents, as well as the inconvenience of use and difficulty in uniform mixing due to the large number of gel formulation components, which affect the field application effect, the present invention aims to provide a thermally associative gel for sealing that has high associative structural strength and good stability at high temperatures, as well as its preparation method and application.

[0010] To achieve the above objectives, the first aspect of the present invention provides a thermoassociated gel, the raw materials of which include alkenylamide monomers, functional monomers, crosslinking agents and initiators;

[0011] The functional monomer is selected from at least two of alkenyl hydrophobic monomers, alkenyl cyclic monomers, and alkenyl sulfonic acid monomers.

[0012] According to a specific embodiment of the present invention, the amount of the alkenylamide monomer is 10 to 12 parts by mass, the amount of the functional monomer is 8 to 10 parts by mass, the amount of the crosslinking agent is 0.3 to 0.6 parts by mass, and the amount of the initiator is 0.03 to 0.05 parts by mass.

[0013] Preferably, the amount of the alkenylamide monomer is 10.1 to 11.7 parts by weight, the amount of the functional monomer is 8.3 to 9.9 parts by weight, the amount of the crosslinking agent is 0.35 to 0.55 parts by weight, and the amount of the initiator is 0.03 to 0.05 parts by weight.

[0014] According to a specific embodiment of the present invention, the alkenylamide monomer is selected from two of acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide and N-isopropylacrylamide;

[0015] and / or

[0016] The alkenyl hydrophobic monomer is selected from one of dimethyldiallylhexadecylammonium chloride, N-hexadecylacrylamide, and N-octadecylacrylamide; and / or

[0017] The alkenyl cyclic monomer is vinylpyrrolidone; and / or

[0018] The alkenyl sulfonic acid monomer is selected from 2-acrylamide-2-methylpropanesulfonic acid and / or methylpropanesulfonic acid;

[0019] and / or

[0020] The crosslinking agent is at least one selected from cyclohexamethylenetetramine, hydroquinone, phenolic resin, zirconium acetate, and p-phthalaldehyde; and / or

[0021] The initiator is at least one of potassium persulfate, ammonium persulfate, and azobisisobutylamidine hydrochloride.

[0022] According to a specific embodiment of the present invention, the functional monomer includes an alkenyl hydrophobic monomer and an alkenyl sulfonic acid monomer;

[0023] Preferably, the functional monomer is 100% by mass, and the functional monomer comprises 30.8 wt% to 34 wt% of the alkenyl hydrophobic monomer and 66 wt% to 69.2 wt% of the alkenyl sulfonic acid monomer.

[0024] According to a specific embodiment of the present invention, the functional monomer includes the alkenyl hydrophobic monomer and the alkenyl cyclic monomer;

[0025] Preferably, the functional monomer is 100% by mass, and the functional monomer comprises 42 wt% of the alkenyl hydrophobic monomer and 58 wt% of the alkenyl cyclic monomer.

[0026] A second aspect of the present invention provides a method for preparing a thermoassociated gel as described in the first aspect of the present invention, comprising the following steps:

[0027] 1) The alkenylamide monomer, functional monomer, crosslinking agent and first solvent are mixed to obtain a monomer-crosslinking agent solution;

[0028] 2) The monomer-crosslinking agent solution is reacted under the action of the initiator and dried to obtain the thermally associative gel.

[0029] According to one specific embodiment of the present invention, the first solvent is water.

[0030] According to a specific embodiment of the present invention, in step 1), the pH of the monomer-crosslinking agent solution is adjusted to neutral before proceeding to step 2); and / or

[0031] In step 2), the reaction solution obtained from the reaction is purified and then dried.

[0032] Preferably, the pH is adjusted with sodium hydroxide (e.g., a 20 wt% aqueous solution of sodium hydroxide);

[0033] Preferably, the purification involves precipitating the reaction solution with a second solvent, filtering, collecting the filter residue, and then drying it; and / or

[0034] The second solvent is ethanol and / or acetone.

[0035] According to one specific embodiment of the present invention, the reaction conditions are: reacting at 60°C to 65°C for 6 to 8 hours; and / or

[0036] The drying temperature is 65°C to 75°C; and / or the duration is 18h to 24h.

[0037] Preferably, the reaction is carried out under anaerobic conditions.

[0038] The application of the thermally associative gel according to the first aspect of the present invention or the thermally associative gel prepared by the method according to the second aspect of the present invention in the plugging of high-temperature fractured-vuggy reservoirs, especially as a plugging agent;

[0039] Preferably, the high temperature reaches a maximum of 140°C.

[0040] The beneficial effects of this invention are:

[0041] To address the problems of low structural strength and limited temperature resistance in existing polymer gel sealing agents, as well as the inconvenience of use and difficulty in uniform mixing due to the large number of gel formulation components, which affects the field performance, this invention provides a thermoassociated gel, its preparation method, and its application. The thermoassociated gel is obtained by reacting alkenylamide monomers, functional monomers, and crosslinking agents under the action of an initiator, and has the advantages of high structural strength, good high-temperature resistance, and good sealing performance.

[0042] (1) The thermally associative gel has a structural strength of about 3500 Pa to 3750 Pa at 140 °C, and has high structural strength at high temperature.

[0043] (2) The thermal associative gel at 140℃ and 3.5MPa has a leakage of 64 to 82 mL when sealing a 1 mm wide crack for 0.5 h, a leakage of 56 to 84 mL when sealing a 2 mm wide crack for 0.5 h, and a leakage of 52 to 72 mL when sealing a 3 mm wide crack for 0.5 h. The leakage is relatively small when sealing cracks of 1 to 3 mm wide, and the sealing effect is good.

[0044] (3) The thermally associative gel has a sealing strength of 8 MPa for cracks 1 to 3 mm wide at 140°C and can maintain a sealing pressure of 8 MPa for at least 1 hour, achieving a long-term effective sealing effect at high temperature.

[0045] The thermally associative gel has fewer raw material types, a simple preparation method, and is already a finished product before entering the formation. It overcomes the problems of existing technologies, such as a large number of gel components, inconvenience in use, and difficulty in uniform mixing, which affect the sealing effect. It can be used as a plugging agent to effectively seal fractured-vuggy reservoirs at temperatures up to 140°C. Attached Figure Description

[0046] Figure 1 The graphs show the changes in shear force with shear time during the thermal associative performance evaluation experiments of the thermally associative gels prepared in Examples 1 to 3. Detailed Implementation

[0047] The present invention will be further described below with reference to the embodiments. However, the embodiments of the present invention are merely illustrative examples and should not be construed as limiting the present invention under any circumstances.

[0048] Example 1

[0049] 1) Weigh 4.25g of acrylamide, 5.88g of N-isopropylacrylamide, 3.35g of dimethyldiallylhexadecylammonium chloride, 6.52g of 2-acrylamido-2-methylpropanesulfonic acid, 0.15g of zirconium acetate and 0.2g of hydroquinone, mix with 200mL of deionized water, stir well to obtain monomer-crosslinking agent solution;

[0050] 2) Adjust the pH of the monomer-crosslinking agent solution to neutral with 20wt% sodium hydroxide aqueous solution, add 0.05g of potassium persulfate, purge oxygen with nitrogen for 20min, raise the water bath temperature to 60℃, react for 8h, precipitate the reaction solution with ethanol, filter, collect the filter residue, dry at 60℃ for 18h, pulverize, and obtain the thermally associative gel sealing agent.

[0051] Example 2

[0052] 1) Weigh 5.38g of acrylamide, 6.35g of N,N-diethylacrylamide, 2.55g of N-octadecylacrylamide, 5.72g of methylpropanesulfonic acid, 0.4g of cyclohexamethylenetetramine and 0.15g of phenol, mix with 200mL of deionized water, stir evenly to obtain monomer-crosslinking agent solution;

[0053] 2) Adjust the pH of the monomer-crosslinking agent solution to neutral with 20% sodium hydroxide aqueous solution, add 0.03g of azobisisobutylamidine hydrochloride, purge oxygen with nitrogen for 20min, raise the water bath temperature to 63℃, react for 6h, precipitate the reaction solution with acetone, filter, collect the filter residue, dry at 70℃ for 20h, pulverize, and obtain the thermally associative gel sealing agent.

[0054] Example 3

[0055] 1) Weigh 6.42g of N,N-dimethylacrylamide, 5.15g of N-isopropylacrylamide, 3.55g of N-hexadecylacrylamide, 4.88g of vinylpyrrolidone, 0.25g of cyclohexamethylenetetramine and 0.3g of p-phthalaldehyde, mix with 200mL of deionized water, stir well to obtain monomer-crosslinking agent solution;

[0056] 2) Adjust the pH of the monomer-crosslinking agent solution to neutral with 20% sodium hydroxide aqueous solution, add 0.03g of azobisisobutylamidine hydrochloride, purge oxygen with nitrogen for 20min, raise the water bath temperature to 65℃, react for 8h, precipitate the reaction solution with acetone, filter, collect the filter residue, dry at 75℃ for 24h, pulverize, and obtain the thermally associative gel sealing agent.

[0057] Performance evaluation of thermoassociated gel

[0058] 1. Evaluation of thermal association

[0059] The structural strength of the thermally associative gels prepared in Examples 1 to 3 after hydration was measured to evaluate their thermal associative properties. The specific steps are as follows:

[0060] i. First, weigh 100 mL of water into a 250 mL beaker. Then, weigh 5 g of the thermoassociated gel prepared in any one of Examples 1 to 3 and add it to the beaker containing 100 mL of water. Place it at room temperature for 24 h to hydrate and obtain the hydrated thermoassociated gel.

[0061] ii. Using a HAAKE RS6000 high-temperature and high-pressure rheometer at 140°C and normal pressure, the rheometer was used to measure the rheometry results in a 10-second pulse. -1 The shear rate was measured, and the structural strength of the hydrated thermoassociated gel obtained in step i was determined.

[0062] Following the above method, the structural strength of the thermally associated gels prepared in Examples 1 to 3 was measured after hydration.

[0063] For details, please see [link / details]. Figure 1 .

[0064] Figure 1 This reflects the change in shear force with shear time during the experiment of the thermally associating gels prepared in Examples 1 to 3 after hydration. It can be seen that with increasing shear time, the shear force rapidly rises to a peak value and then rapidly decreases, eventually stabilizing. The peak value reached by the shear force during the increase of shear time represents the structural strength of the thermally associating gel. As shown in the figure, the structural strength of the thermally associating gels prepared in Examples 1 to 3 is approximately 3500 to 3750 Pa, exhibiting high structural strength. This demonstrates that the thermally associating gels prepared in Examples 1 to 3 have good thermal associative properties, which helps them to effectively seal leaks under high-temperature conditions.

[0065] 2. Evaluation of Leak-Plugging Performance

[0066] The thermally associative gels prepared in Examples 1 to 3 were used to seal cracks of different widths at high temperatures to evaluate the sealing performance of the thermally associative gels at high temperatures.

[0067] The specific steps are as follows:

[0068] Testing instrument: UDL-150-10 high temperature and high pressure leak sealing instrument;

[0069] Experimental temperature: 140℃;

[0070] A. Weigh 100 mL of water into a 250 mL beaker, then weigh 5 g of the thermoassociated gel prepared in any one of Examples 1 to 3, add it to the beaker containing 100 mL of water, and hydrate it at room temperature for 24 h to obtain the hydrated thermoassociated gel.

[0071] B. First, measure and record the leakage of the hydrated thermoassociated gel prepared in step A when sealing cracks with widths of 1 mm, 2 mm, and 3 mm at a pressure of 3.5 MPa and an experimental time of 0.5 h.

[0072] C. Then, the pressure is gradually increased from 3.5 MPa at a rate of 0.5 MPa per hour. After each increase of 0.5 MPa, the pressure is stabilized for 1 hour. If no sudden drop in experimental pressure occurs, the pressure-bearing capacity of the thermally associative gel when sealing cracks with widths of 1 mm, 2 mm, and 3 mm at 140℃ can be obtained.

[0073] Following steps A, B, and C, experiments were conducted using the thermally associative gels prepared in Examples 1 to 3, respectively.

[0074] The specific results are shown in Tables 1 and 2.

[0075] Table 1. Leakage of thermoassociated gel at 140℃, 3.5MPa, and 0.5h

[0076]

[0077] Table 2. Pressure resistance of thermoassociated gel for sealing cracks of different widths

[0078]

[0079] As shown in Table 1, the thermally associative gels prepared in Examples 1 to 3, under the conditions of 140℃, 3.5MPa, and a sealing time of 0.5h, exhibited the following leakage rates: 64 to 82 mL for sealing a 1 mm wide crack, 56 to 84 mL for sealing a 2 mm wide crack, and 52 to 72 mL for sealing a 3 mm wide crack. These data indicate that the thermally associative gels prepared in Examples 1 to 3 exhibited low leakage when sealing 1 to 3 mm wide cracks at a high temperature (140℃), demonstrating good sealing performance for cracks ranging from 1 to 3 mm wide at 140℃.

[0080] As can be seen from the data in Table 2, the thermally associating gels prepared in Examples 1 to 3 all achieved a sealing strength of 8 MPa for 1 mm wide, 2 mm wide, and 3 mm wide cracks at 140°C, and all could maintain a sealing pressure of 8 MPa for at least 1 hour. This indicates that the thermally associating gels prepared in Examples 1 to 3 can achieve continuous, effective, and stable sealing of 1 to 3 mm wide cracks at a high temperature of 140°C, meeting the requirements for long-term high-temperature resistance.

[0081] Based on the experimental results of the thermal associative performance evaluation and leakage plugging performance evaluation of the thermally associative gels prepared in Examples 1 to 3, it can be concluded that the thermally associative gels prepared in Examples 1 to 3 have high structural strength and high strength performance in continuously and stably plugging 1 to 3 mm wide fractures under high temperature conditions of 140℃. They can be applied in leakage plugging operations of fracture-vuggy high-temperature oil reservoirs in the Tahe carbonate rock, which is of great significance for the efficient drilling and development of deep carbonate rock oil reservoirs in the Tahe.

[0082] While the present invention has been described with reference to specific embodiments, those skilled in the art will understand that various changes can be made without departing from the true spirit and scope of the invention. Furthermore, numerous modifications can be made to the subject, spirit, and scope of the invention to suit specific situations, materials, material compositions, and methods. All such modifications are included within the scope of the claims of the present invention.

Claims

1. A thermoassociated gel, the raw materials of which include alkenylamide monomers, functional monomers, crosslinking agents and initiators; The functional monomers are a combination of an alkenyl hydrophobic monomer and an alkenyl sulfonic acid monomer, the mass of the functional monomers being 100%, the mass of the alkenyl hydrophobic monomer being 30.8wt% to 34wt%, and the mass of the alkenyl sulfonic acid monomer being 66wt% to 69.2wt%; or the functional monomers are a combination of the alkenyl hydrophobic monomer and an alkenyl cyclic monomer, the mass of the functional monomers being 100%, the mass of the alkenyl hydrophobic monomer being 42wt%, and the mass of the alkenyl cyclic monomer being 58wt%; wherein, The amount of the alkenylamide monomer is 10 to 12 parts by weight, the amount of the functional monomer is 8 to 10 parts by weight, the amount of the crosslinking agent is 0.3 to 0.6 parts by weight, and the amount of the initiator is 0.03 to 0.05 parts by weight.

2. Thermotropic gel according to claim 1, characterized in that The alkenylamide monomer is selected from two of acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, and N-isopropylacrylamide; and / or The alkenyl hydrophobic monomer is selected from one of dimethyldiallylhexadecylammonium chloride, N-hexadecylacrylamide, and N-octadecylacrylamide; and / or The alkenyl cyclic monomer is vinylpyrrolidone; and / or The alkenyl sulfonic acid monomer is selected from 2-acrylamido-2-methylpropanesulfonic acid and / or methylpropanesulfonic acid; and / or The crosslinking agent is at least one selected from cyclohexamethylenetetramine, hydroquinone, phenolic resin, zirconium acetate, and p-phthalaldehyde; and / or The initiator is at least one of potassium persulfate, ammonium persulfate, and azobisisobutylamidine hydrochloride.

3. A method for preparing the thermoassociated gel as described in claim 1 or 2, comprising the following steps: 1) The alkenylamide monomer, functional monomer, crosslinking agent and first solvent are mixed to obtain a monomer-crosslinking agent solution; 2) The monomer-crosslinking agent solution is reacted under the action of the initiator and dried to obtain the thermally associative gel.

4. The method of claim 3, wherein, The first solvent is water.

5. The method according to claim 3, characterized in that, In step 1), the monomer-crosslinking agent solution is adjusted to neutral pH before proceeding to step 2); and / or In step 2), the reaction solution obtained from the reaction is purified and then dried. Adjust the pH with sodium hydroxide; The purification process involves precipitating the reaction solution with a second solvent, filtering, collecting the filter residue, and then drying it. and / or The second solvent is ethanol and / or acetone.

6. The method according to any one of claims 3 to 5, characterized in that, The reaction is carried out at 60°C to 65°C for 6 to 8 hours under anaerobic conditions.

7. The application of the thermally associating gel according to claim 1 or 2, or the thermally associating gel prepared by any one of claims 3 to 6, in the plugging of high-temperature fractured-vuggy reservoirs.

8. The application according to claim 7, characterized in that, The application refers to the use of the thermally associative gel as a plugging agent in the sealing of high-temperature fractured reservoirs; the highest temperature is 140°C.

Citation Information

Patent Citations

  • Gel cement, associated polymer and preparation method

    CN111268953A

  • Method for preparing high-temperature cross-linking plugging agent for high-permeability oil reservoir recovery