Hydrogenated bio-based terpene binary random copolymerized elastomer as well as preparation method and application thereof
Through the preparation of hydrogenated bio-based terpene two-member random copolymer elastomers, the bottleneck of the POE industry development and insufficient performance of bio-based materials have been solved, and high-performance hydrogenated bio-based terpene two-member random copolymer elastomers are realized. In a variety of application areas and reduces hydrogenation costs.
Patent Information
- Application Number
- CN202411198760.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
There are bottlenecks in the development of the existing POE industry, the comprehensive performance of bio-based materials is not high, and the research on hydrogenated terpene polymers has not been involved, which cannot effectively alleviate environmental problems and domestic application demand for POE elastomers.
Develop a hydrogenated bio-based terpene two-membered random copolymer elastomer. Through the copolymerization and hydrogenation of bio-based monoterpene and sesquiterpene, hydrogenated bio-based terpene without carbon and hydrocarbon double bonds and having long side chains are prepared. Two-member random copolymer elastomer is hydrogenated using Ziegler-Natta hydrogenation reaction system or metallocene hydrogenation reaction system to optimize the hydrogenation process to improve the overall hydrogenation degree.
It has achieved high light transmittance, aging resistance and high elongation of break of hydrogenated bio-based terpene two-member random copolymer elastomer, which is suitable for a variety of application fields, and has excellent impact resistance and processing properties similar to POE. , reduces hydrogenation costs and is suitable for industrial production.
Smart Images

Figure CN119060253A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of olefin catalytic polymerization and hydrogenation, and specifically relates to a hydrogenated bio-based terpene binary random copolymer elastomer and a preparation method and application thereof. Background Art
[0002] With the reduction of fossil energy and people's increasing awareness of environmental protection, it is increasingly important to develop new sustainable bio-based energy in a timely manner and use bio-based energy to synthesize polymer materials to replace petroleum derivatives. Among them, bio-based terpenes belong to a type of currently popular sustainable bio-based energy. It is a type of natural molecular biomass rich in hydrocarbons. The main components of resins produced by many plants, such as pine and coniferous trees, contain terpenes. Most terpenes have a basic alicyclic structure and an isoprene basic unit. They can be classified into hemiterpenes, monoterpenes, sesquiterpenes, diterpenes, dipterpenes, triterpenes, etc. according to the number of isoprenes they contain. These terpenes can be used as monomers for various polymerization reactions.
[0003] In modern society, the public's demand for high-end life and daily chemical products has also become higher. At present, the consumption in various application fields such as various films, auto parts, medical packaging materials, wires and cables, daily products and toys, and stretchable materials or flexible stretchable energy storage devices in China has gradually increased, and the polymer materials used to produce these consumer products are mainly POE. POE is a type of copolymer formed by the copolymerization of ethylene and octene. The molecular chain does not contain carbon-hydrogen double bonds and has a long side chain. According to market consumption, although my country is a major consumer of POE, the current development of POE-related products in my country is not perfect and still faces severe challenges. It is necessary to solve the current development difficulties as soon as possible. At this stage, the research on hydrogenated polymers has not yet involved hydrogenated terpene polymers, which have high researchability and development potential. Therefore, in response to the increasingly serious environmental problems facing the world, it is necessary to develop a new type of bio-based material to alleviate the domestic application demand for POE elastomers, and at the same time make full use of existing bio-based resources. Summary of the invention
[0004] The purpose of the present invention is to solve the bottleneck of POE industry development and the technical problem of low comprehensive performance of bio-based materials, and to provide a hydrogenated bio-based terpene binary random copolymer elastomer and its preparation method and application.
[0005] The technical solution of the present invention is as follows:
[0006] One of the purposes of the present invention is to provide a hydrogenated bio-based terpene binary random copolymer elastomer, which is prepared by copolymerizing and hydrogenating bio-based monoterpene and bio-based sesquiterpene, wherein the molar content of monoterpene polymerization units is 5 to 95%, the molar content of sesquiterpene polymerization units is 5 to 95%, the degree of hydrogenation is 90% to 99.9%, the number average molecular weight is 10,000 to 500,000 g / mol, and the molecular weight distribution is 1.0 to 5.0.
[0007] Preferably, the monoterpene is one or more of geraniol, limonene, α-myrcene, β-myrcene, β-citronellol, citral, and menthol, and the sesquiterpene is one or more of cadinene, α-farnesene, β-farnesene, cedrene, and caryophyllene.
[0008] More preferably, the monoterpene is β-myrcene and the sesquiterpene is β-farnesene.
[0009] Preferably, the hydrogenated bio-based terpene binary random copolymer elastomer has a molar content of monoterpene polymerization units of 10 to 90%, a molar content of sesquiterpene polymerization units of 10 to 90%, a degree of hydrogenation of 96 to 99%, and a molecular weight distribution of 1.9 to 3.1.
[0010] Preferably, the hydrogenated bio-based terpene binary random copolymer elastomer has a glass transition temperature range of -80 to -50°C.
[0011] Further preferably, the hydrogenated bio-based terpene binary random copolymer elastomer has a glass transition temperature range of -69 to -60°C.
[0012] Preferably, the elongation at break of the hydrogenated bio-based terpene binary random copolymer elastomer is greater than 800%, and the volume resistivity is greater than 0.6×10 18 Ω.cm, melt index is 65-85g / 10min, light transmittance at 380-1100nm is 85-99%, water vapor transmission is 2-3.9%, low temperature notched impact strength at -30℃ is 50-70KJ / m 2 , cantilever beam notch impact strength is 10~20KJ / m 2 , the heat deformation temperature is 130~160℃.
[0013] Further preferably, the elongation at break of the hydrogenated bio-based terpene binary random copolymer elastomer is greater than 850%, and the volume resistivity is greater than 0.78×10 18 Ω.cm, melt index is 69-76g / 10min, light transmittance at 380-1100nm is 89-94%, water vapor transmission is 2.5-3.1%, low temperature notched impact strength at -30℃ is 59-65KJ / m 2 , cantilever beam notch impact strength is 13.7~15.1KJ / m2 , the heat deformation temperature is 139~151℃.
[0014] The second object of the present invention is to provide a method for preparing a hydrogenated bio-based terpene binary random copolymer elastomer, characterized in that the method:
[0015] (1) preparing a binary random copolymer by copolymerizing bio-based monoterpene and bio-based sesquiterpene monomers;
[0016] (2) The binary random copolymer is dissolved in a solvent to obtain a copolymer solution, and then hydrogenated using a Ziegler-Natta hydrogenation reaction system or a metallocene hydrogenation reaction system to obtain a hydrogenated bio-based terpene binary random copolymer elastomer.
[0017] Preferably, the copolymerization in step (1) is carried out by anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization.
[0018] More preferably, the specific process of anionic polymerization is as follows:
[0019] The copolymerization is initiated under anhydrous and oxygen-free conditions with an organic alkali metal as an initiator and / or an organic aluminum compound as a co-catalyst.
[0020] More preferably, the organic alkali metal is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, methyllithium, ethyllithium, n-propyllithium, isopropyllithium, phenyllithium, benzyllithium, and naphthalenelithium; the organic aluminum compound can be abbreviated as AB, wherein A represents one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, and sesquiethylaluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, 2,6-di-tert-butylphenol, 2-tert-butylphenol, and 2,6-di-tert-butyl-4-ethylphenol; the reaction temperature is -50°C to 70°C, and the reaction time is 10 to 360 min.
[0021] Preferably, the coordination polymerization method includes iron coordination polymerization, Zignata-type catalyst system polymerization, cationic lutetium coordination complex polymerization with β-diaminosulfonate as ligand, rare earth lanthanum catalyst polymerization system polymerization, [OSSO] type titanium complex polymerization, half sandwich scandium complex polymerization, and cobalt catalyst system polymerization.
[0022] Further preferably, the specific process of using the iron coordination polymerization method is:
[0023] Under anhydrous and oxygen-free conditions, an iron catalyst, a co-catalyst, bio-based monoterpene and bio-based sesquiterpene monomers and a solvent are added into a reactor, and a polymerization reaction is carried out at 0 to 100° C. with stirring for 10 to 120 minutes.
[0024] More preferably, the iron catalyst is any one of the following structural formulas:
[0025]
[0026] Preferably, the concentration of the copolymer solution in step (2) is 10 wt %, and the solvent of the copolymer solution is one or more of toluene, xylene, n-hexane, and cyclohexane.
[0027] Preferably, the Ziegler-Natta hydrogenation reaction process in step (2) is:
[0028] Under an argon atmosphere, add a mixed liquid of the copolymer solution, the catalyst and the co-catalyst into a dry high-temperature reactor, replace the gas in the reactor three times with hydrogen, adjust the reactor speed to 200-600 rpm, the hydrogenation reaction pressure to 1-4 MPa, increase the temperature to 45-70°C, and react for 1-3 hours.
[0029] Further preferably, the catalyst is one or more of titanium dioxide, titanium sulfate, titanium hydroxide, nickel cyclohexaneate, nickel bromide, nickel cobalt, and nickel fluoride, the co-catalyst is an organic metal compound of a metal from Group IA to Group IIIA, the mass ratio of the copolymer to the catalyst in the copolymer solution is (1 to 300):1, and the molar ratio of the catalyst to the co-catalyst is 1:(1 to 10).
[0030] More preferably, the catalyst is titanium sulfate or nickel naphthenate, and the co-catalyst is one or more of aluminum acetate, aluminum hydroxide, sesquiethylaluminum chloride, DMAO, and MMAO.
[0031] Preferably, the metallocene hydrogenation reaction system in step (2) comprises a bis(titanocenes) / lithium hydride / aromatic ester system, a bis(titanocenes) or mono(titanocenes) / triphenyllithium system, a bis(titanocenes) / alkylaluminum / silicate system or a bis(titanocenes) / alkylaluminum / lithium-based metal compound system.
[0032] More preferably, the specific process of hydrogenation using the bis(triocene)titanium / alkylaluminum / lithium metal compound system is as follows:
[0033] Under an argon atmosphere, the copolymer solution and the diocene titanocene / alkyl aluminum / lithium metal compound composite catalyst were added in sequence to a dry high-temperature reactor. The gas in the reactor was replaced three times with hydrogen. The speed of the reactor was adjusted to 200-800 rpm, the hydrogenation reaction pressure was 2.5-3.0 MPa, the temperature was increased to 50-80°C, and the reaction was carried out for 0.1-1.5 hours.
[0034] More preferably, the catalyst bis(titanocenes) comprises dichlorobis(titanocenes); the co-catalyst alkylaluminum is one or more of aluminum chloride, diethylaluminum chloride, tri-n-hexylaluminum, dimethylaluminum chloride, trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, and diisobutylaluminum hydride; the lithium-based metal compound is one or more of lithium fluoride, lithium carbonate, lithium phosphate, lithium nitride, lithium hydroxide, and lithium chloride; the mass ratio of the copolymer and the bis(titanocenes) in the copolymer solution is (1 to 5000):1; the molar ratio of the bis(titanocenes) to the alkylaluminum is 1:(1 to 6); and the molar ratio of the bis(titanocenes) to the lithium-based metal compound is 1:(1 to 8).
[0035] The third object of the present invention is to provide an application of the above-mentioned hydrogenated bio-based terpene binary random copolymer elastomer in the preparation of hot melt adhesives and film products used in photovoltaic solar energy and batteries, automotive interiors, clothing, footwear, electronics, wall coverings, construction, filtration or medical fields.
[0036] Compared with the prior art, the present invention has the following advantages:
[0037] (1) The present invention uses a bio-based monoterpene monomer with a glass transition temperature of less than -65°C and a bio-based sesquiterpene monomer with a glass transition temperature of less than -70°C to perform random copolymerization to obtain a two-component random copolymer, and then hydrogenates the two-component random copolymer product to obtain a hydrogenated bio-based terpene two-component random copolymer elastomer that does not contain a carbon-hydrogen double bond and has a relatively long side chain. The hydrogenated product has good light transmittance, aging resistance and high elongation at break, and can be used to produce hot melt adhesive films and hot melt adhesives used in photovoltaic solar energy and batteries, automotive interiors, clothing, shoe materials, electronics, wall coverings, construction, filtration, medicine and other fields.
[0038] (2) The hydrogenated bio-based terpene binary random copolymer elastomer of the present invention has a carbon-carbon single bond ratio of more than 90%, and its weather resistance, mechanical strength and ductility are relatively excellent. The elastomer is similar to the POE elastomer in structure and contains a longer side chain, so it has better impact resistance than POE. At the same time, it has excellent processing and use performance like POE. And because the side chain is longer, its elastic deformation recovery ability is stronger.
[0039] (3) The polymerization pathway proposed in the present invention has the characteristics of easy availability of raw materials, simple operation, and environmentally friendly components. The system has high catalytic activity and a monomer conversion rate of more than 90%. At the same time, the hydrogenation process is optimized to further reduce the hydrogenation cost. The overall hydrogenation degree of the polymer reaches more than 95%, which is suitable for industrial production and alleviates dependence on POE products. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The bio-based terpene binary random copolymer obtained in Example 1 1 H NMR spectrum;
[0041] Figure 2 The hydrogenated bio-based terpene binary random copolymer elastomer obtained in Example 1 1 H NMR spectrum;
[0042] Figure 3 This is the GPC spectrum of the hydrogenated bio-based terpene binary random copolymer elastomer obtained in Example 1;
[0043] Figure 4 This is the DSC spectrum of the hydrogenated bio-based terpene binary random copolymer elastomer obtained in Example 1. DETAILED DESCRIPTION
[0044] The invention provides a hydrogenated bio-based terpene binary random copolymer elastomer, wherein the hydrogenated bio-based terpene binary random copolymer elastomer is prepared by copolymerizing and hydrogenating bio-based monoterpene and bio-based sesquiterpene, wherein the molar content of monoterpene polymerization units is 5-95%, the molar content of sesquiterpene polymerization units is 5-95%, the degree of hydrogenation is 90%-99.9%, the number average molecular weight is 10,000-500,000 g / mol, and the molecular weight distribution is 1.0-5.0.
[0045] Preferably, the monoterpene is one or more of geraniol, limonene, α-myrcene, β-myrcene, β-citronellol, citral, and menthol, and β-myrcene is more preferably used; the sesquiterpene is one or more of cadinene, α-farnesene, β-farnesene, cedrene, and caryophyllene, and β-farnesene is more preferably used.
[0046] Preferably, the hydrogenated bio-based terpene binary random copolymer elastomer has a molar content of monoterpene polymerization units of 10 to 90%, a molar content of sesquiterpene polymerization units of 10 to 90%, a degree of hydrogenation of 96 to 99%, and a molecular weight distribution of 1.9 to 3.1.
[0047] Preferably, the hydrogenated bio-based terpene binary random copolymer elastomer has a glass transition temperature in the range of -80 to -50°C, more preferably in the range of -69 to -60°C.
[0048] Preferably, the elongation at break of the hydrogenated bio-based terpene binary random copolymer elastomer is greater than 800%, and the volume resistivity is greater than 0.6×10 18 Ω.cm, melt index is 65-85g / 10min, light transmittance at 380-1100nm is 85-99%, water vapor transmission is 2-3.9%, low temperature notched impact strength at -30℃ is 50-70KJ / m 2 , cantilever beam notch impact strength is 10~20KJ / m 2, and the heat deformation temperature is 130-160°C. Further preferably, the elongation at break of the hydrogenated bio-based terpene binary random copolymer elastomer is greater than 850%, and the volume resistivity is greater than 0.78×10 18 Ω.cm, melt index is 69-76g / 10min, light transmittance at 380-1100nm is 89-94%, water vapor transmission is 2.5-3.1%, low temperature notched impact strength at -30℃ is 59-65KJ / m 2 , cantilever beam notch impact strength is 13.7~15.1KJ / m 2 , the heat deformation temperature is 139~151℃.
[0049] The present invention also provides a method for preparing a hydrogenated bio-based terpene binary random copolymer elastomer, the method being carried out according to the following steps:
[0050] (1) preparing a binary random copolymer by copolymerizing bio-based monoterpene and bio-based sesquiterpene monomers;
[0051] (2) The binary random copolymer is dissolved in a solvent to obtain a copolymer solution, and then hydrogenated using a Ziegler-Natta hydrogenation reaction system or a metallocene hydrogenation reaction system to obtain a hydrogenated bio-based terpene binary random copolymer elastomer.
[0052] Preferably, the preparation of the binary random copolymer in step (1) is carried out by anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization. More preferably, it is coordination polymerization, anionic polymerization or free radical polymerization. More preferably, it is coordination polymerization or anionic polymerization.
[0053] Preferably, the coordination polymerization method includes iron coordination polymerization, Zignata type catalyst system polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, half sandwich scandium complex polymerization, cobalt catalyst system polymerization. More preferably, it is iron coordination polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, cobalt catalyst system polymerization. More preferably, it is iron coordination polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization. Most preferably, it is iron coordination polymerization.
[0054] Preferably, when the preparation of the binary random copolymer adopts the iron coordination polymerization method, the specific steps are: under anhydrous and oxygen-free conditions, add an iron catalyst, a co-catalyst, bio-based monoterpene and bio-based sesquiterpene monomers and a solvent into a reactor, and stir the polymerization reaction at 0 to 100° C. for 10 to 120 minutes.
[0055] Preferably, the iron catalyst is any one of the following structural formulas:
[0056]
[0057] More preferably, the reaction temperature is 0-30° C. and the reaction time is 30 min.
[0058] Further preferably, the solvent is one or more of cyclohexane, n-hexane, petroleum ether, toluene, and xylene, and the ratio of the solvent to the total volume of the comonomer is (1-50):1, more preferably (3-10):1; the molar ratio of the total molar amount of the comonomer to the iron element in the iron catalyst is (100-50000):1, more preferably (155-20000):1.
[0059] Further preferably, the co-catalyst is a single component or a two-component. When the co-catalyst is a single component, the co-catalyst is selected from one or more of methylaluminoxane (MAO), dried methylaluminoxane (DMAO), and modified methylaluminoxane (MMAO). The molar ratio of the aluminum element in the co-catalyst to the iron element in the iron catalyst is (100-1500):1, more preferably 500:1; when the co-catalyst is a two-component, component A is selected from one or more of trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, diisobutylaluminum hydride, and sesquiethylaluminum chloride. , component B is one or more of methylaluminoxane (MAO), dried methylaluminoxane (DMAO), modified methylaluminoxane (MMAO), N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, 4-isopropyl-4'-methyldiphenyl iodide tetrakis(pentafluorophenyl)borate, triphenylphosphine oxide, tris(pentafluorophenyl)phosphine, and triphenylphosphine, the molar ratio of aluminum element in component A to iron element in the iron catalyst is (1-100):1, more preferably 40:1, and the molar ratio of aluminum, boron or phosphine element in component B to iron element in the iron catalyst is (1-20):1, more preferably 1:1.
[0060] When the preparation of the binary random copolymer adopts anionic polymerization, the specific steps are: under anhydrous and oxygen-free conditions, an organic alkali metal is used as an initiator to initiate copolymerization of bio-based monoterpene and bio-based sesquiterpene monomers, and after reacting at a certain temperature for a certain time, ethanol is added to quench the reaction and obtain a polymerization product;
[0061] Alternatively, under anhydrous and oxygen-free conditions, an organic alkali metal is used as an initiator and an organic aluminum compound is used as a co-catalyst to initiate the copolymerization of bio-based monoterpene and bio-based sesquiterpene monomers. After reacting at a certain temperature for a certain time, ethanol is added to quench the reaction and obtain a polymerization product.
[0062] Preferably, the organic alkali metal is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, methyllithium, ethyllithium, n-propyllithium, isopropyllithium, phenyllithium, benzyllithium, and naphthalenelithium; more preferably, it is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, and n-propyllithium.
[0063] Preferably, the reaction temperature is -50°C to 70°C, and the reaction time is 10 to 360 min; more preferably, the reaction temperature is 25°C, and the reaction time is 30 min.
[0064] Preferably, the solvent is one or more of THF, toluene, ethylbenzene, xylene, n-hexane, cyclohexane, dichloromethane, chloroform, ethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and methyl tert-butyl ether; further preferably, the solvent is one or more of THF, toluene, ethylbenzene, n-hexane, cyclohexane, ethylene glycol dimethyl ether, and methyl tert-butyl ether.
[0065] Preferably, the organoaluminum compound can be abbreviated as AB, wherein A represents one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, and sesquiethylaluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, 2,6-di-tert-butylphenol, 2-tert-butylphenol, and 2,6-di-tert-butyl-4-ethylphenol, and the molar ratio of A to B is (0.1 to 2):1.
[0066] Preferably, the ratio of the total volume of the solvent to the comonomer is 3:1; the molar ratio of the total molar amount of the comonomer to the lithium element in the initiator is 1556:1; and the molar ratio of the total molar amount of the comonomer to the aluminum element in the cocatalyst is 195:1.
[0067] When the preparation of the binary random copolymer adopts a free radical polymerization method, examples thereof include: hydrogen peroxide polymerization, emulsion polymerization, nitroxide free radical polymerization (NMP), reversible addition chain transfer polymerization (RAFT), etc. Among these methods, nitroxide free radical polymerization (NMP) and reversible addition chain transfer free radical polymerization are preferred; reversible addition chain transfer free radical polymerization is most preferred, and the initiator is one or more of azobisisobutyronitrile, dibenzoyl peroxide, azobisisoheptanenitrile, azobishydroxyvaleric acid, dimethyl azobisisobutyrate, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, and azoisobutylcyanoformamide.
[0068] When the preparation of the binary random copolymer adopts cationic polymerization, the following methods can be cited: cationic polymerization using a dispersible Lewis acid surfactant combination catalyst (LASC) prepared from ytterbium chloride and sodium alkylbenzene sulfonate surfactant; trifluoromethanesulfonate initiation system, boron trifluoride ether initiation system, etc. Among these methods, the LASC polymerization method is preferred.
[0069] Preferably, the polymerization reaction can be quenched by adding a protic compound such as methanol, a methanol solution of acetic acid or a methanol solution of hydrochloric acid; an aqueous solution of acetic acid or hydrochloric acid to the reaction solution.
[0070] Preferably, the concentration of the copolymer solution in step (2) is 10 wt %.
[0071] Preferably, the solvent of the copolymer solution in step (2) is one or more of toluene, xylene, n-hexane and cyclohexane.
[0072] Preferably, in step (2), when a Ziegler-Natta hydrogenation reaction system is used, the specific process of hydrogenation is:
[0073] In an argon atmosphere, a copolymer solution, a catalyst and a co-catalyst mixture are added to a dry high-temperature reactor, and the gas in the reactor is replaced three times with hydrogen. The reactor speed is adjusted to 200-600rpm, the hydrogenation reaction pressure is 1-4MPa, the temperature is raised to 45-70°C, and the reaction is carried out for 1-3h. After the reaction is completed, the system is cooled to room temperature, anhydrous ethanol is poured in, and the hydrogenated elastomer is separated in the form of a precipitate. The precipitate is placed in a vacuum oven and dried at room temperature to a constant weight to obtain the final hydrogenated bio-based terpene binary random copolymer elastomer.
[0074] Further preferably, the catalyst is one or more of titanium dioxide, titanium sulfate, titanium hydroxide, nickel cyclohexaneate, nickel bromide, nickel cobalt, and nickel fluoride, and is most preferably titanium sulfate or nickel cyclohexaneate; the co-catalyst is an organic metal compound of a metal from Group IA to Group IIIA, and is more preferably one or more of aluminum acetate, aluminum hydroxide, sesquiethylaluminum chloride, DMAO, and MMAO, and is most preferably aluminum hydroxide.
[0075] More preferably, the mass ratio of the copolymer to the catalyst in the copolymer solution is (1-300):1, more preferably 200:1; the molar ratio of the catalyst to the co-catalyst is 1:(1-10), more preferably 1:3.
[0076] Further preferably, the hydrogenation reaction temperature is 60° C., the hydrogenation reaction pressure is 1.5 MPa, the rotation speed of the hydrogenation reactor is 500 rpm, and the hydrogenation reaction time is 1.5 h.
[0077] Preferably, the metallocene hydrogenation reaction system in step (2) comprises a bis(titanocenes) / lithium hydride / aromatic ester system, a bis(titanocenes) or mono(titanocenes) / triphenyllithium system, a bis(titanocenes) / alkylaluminum / silicate system or a bis(titanocenes) / alkylaluminum / lithium-based metal compound system.
[0078] More preferably, the specific process of hydrogenation using the bis(triocene)titanium / alkylaluminum / lithium metal compound system is as follows:
[0079] In an argon atmosphere, the copolymer solution and the diocene titanocene / alkyl aluminum / lithium metal compound composite catalyst are added to a dry high-temperature reactor in sequence, and the gas in the reactor is replaced three times with hydrogen. The speed of the reactor is adjusted to 200-800rpm, the hydrogenation reaction pressure is 2.5-3MPa, the temperature is raised to 50-80°C, and the reaction is carried out for 0.1-1.5h. After the reaction is completed, the system is cooled to room temperature, anhydrous ethanol is poured in, and the hydrogenated elastomer is separated in the form of a precipitate. The precipitate is placed in a vacuum oven and dried at room temperature to a constant weight to obtain the final hydrogenated bio-based terpene binary random copolymer elastomer.
[0080] Further preferably, the catalyst dititanocene includes dititanocene dichloride; the co-catalyst alkylaluminum is one or more of aluminum chloride, diethylaluminum chloride, tri-n-hexylaluminum, dimethylaluminum chloride, trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, and diisobutylaluminum hydride, more preferably aluminum chloride; the lithium-based metal compound is one or more of lithium fluoride, lithium carbonate, lithium phosphate, lithium nitride, lithium hydroxide, and lithium chloride, more preferably lithium hydroxide.
[0081] Further preferably, the mass ratio of the copolymer and the bis(trifluoromethyl)titanium in the copolymer solution is (1-5000):1, more preferably 2500:1; the molar ratio of the bis(trifluoromethyl)titanium and the alkylaluminum is 1:(1-6), more preferably 1:3; the molar ratio of the bis(trifluoromethyl)titanium and the lithium metal compound is 1:(1-8), more preferably 1:5; the hydrogenation reaction temperature is preferably 60°C; the hydrogenation reaction pressure is preferably 2.5 MPa; the rotation speed of the hydrogenation reactor is preferably 500 rpm; and the hydrogenation reaction time is preferably 1 h.
[0082] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0083] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0084] The elongation at break test standard in the following embodiments is: GB / T589-2009;
[0085] The light transmittance test standard is: ASTM D1003-2021;
[0086] The water vapor transmission rate test standard is: GB / T 1037-2021;
[0087] Low temperature notched impact strength test standard: ISO179-1:2010;
[0088] The cantilever beam notched impact strength test standard is: refer to ISO180-2019;
[0089] Thermal deformation temperature detection standard: refer to GB / T1634-2019;
[0090] Ohmmeter: Keithley; Model 6517B, 1000v, 10min.
[0091] Example 1: The steps of preparing a hydrogenated bio-based terpene binary random copolymer elastomer of this example are as follows:
[0092] (1) Polymerization: In an argon atmosphere, anhydrous toluene (12.7 mL), β-farnesene (4 mL, 14 mmol, 1400 equiv.), β-myrcene (0.26 mL, 1.56 mmol, 156 equiv.), MAO reagent (5.0 mmol, 500 equiv.), and iron catalyst 2 (1.0 ml, 10 μmol, 1 equiv.) were added to a 50 mL Schlenk tube in sequence, and the polymerization was carried out at 30° C. for 30 min, and then the reaction was terminated with 25 mL of a mixed solution of methanol and hydrochloric acid (MeOH / HCl volume ratio = 50 / 1) and 1 mL of an antioxidant. After the clear liquid was discarded, the polymer was washed three times with ethanol, and the obtained polymer was placed at 40° C. and dried in vacuum to constant weight to obtain a binary random copolymer.
[0093] (2) Hydrogenation: A xylene mother solution (10 wt%) of the copolymer was prepared in a 100 mL Schlenk tube. The catalyst nickel cyclohexaneate (25 mg, 62.3 μmol, 1 equiv.) and the co-catalyst aluminum hydroxide (14.6 mg, 187 μmol, 3 equiv.) were added to the Schlenk tube in sequence under an argon atmosphere, and the mixture was stirred at 500 rpm for 20 mins. The reactor was dried, and 50.0 mL of the xylene mother solution (10 wt%) of the copolymer and the catalyst and co-catalyst reaction blend solution system were added under an argon atmosphere. H2 was used to replace the gas three times, and the pressure in the reactor was 1.5 MPa after stamping. Stirring was started, the hydrogenation temperature was 60°C, the hydrogenation time was 1.5 h, and the rotation speed was 500 rpm. After the reaction, the hydrogenation reactor was cooled to room temperature, and the pressure was released and the mixture was left to stand for 30 mins before opening the reactor. Anhydrous ethanol was added for post-treatment to obtain a white elastomer.
[0094] Example 2: This example is different from Example 1 in that the addition amount of MAO reagent is (50.0 mmol, 5000 equiv.), iron catalyst 2 is (10.0 ml, 100 μmol, 10 equiv.), and the other steps and parameters are the same as those in Example 1.
[0095] Example 3: This example is different from Example 1 in that the reaction is carried out in a 500 mL Schlenk tube, the amount of anhydrous toluene added is (150 mL), the amount of β-farnesene added is (40 mL, 140.0 mmol, 14000 equiv.), the amount of β-myrcene added is (10 mL, 60 mmol, 6000 equiv.), and the other steps and parameters are the same as in Example 1.
[0096] Example 4: This example is different from Example 1 in that the amount of anhydrous toluene added is (6.3 mL), the amount of β-farnesene added is (2 mL, 7 mmol, 700 equiv.), the amount of β-myrcene added is (1.17 mL, 7 mmol, 700 equiv.), and the other steps and parameters are the same as in Example 1.
[0097] Example 5: This example is different from Example 1 in that the amount of anhydrous toluene added is (8.3 mL), the amount of β-farnesene added is (0.45 mL, 1.6 mmol, 156 equiv.), the amount of β-myrcene added is (2.3 mL, 14 mmol, 1400 equiv.), and the other steps and parameters are the same as in Example 1.
[0098] Example 6: This example is different from Example 1 in that the reaction is carried out in a 100 mL Schlenk tube, the amount of anhydrous toluene added is (43 mL), and the other steps and parameters are the same as in Example 1.
[0099] Example 7: This example is different from Example 1 in that the iron catalyst is replaced with iron catalyst 1, the addition amount is (1.0 ml, 10 μmol, 1 equiv.), and the copolymerization reaction temperature is 0°C; the other steps and parameters are the same as those in Example 1.
[0100] Embodiment 8: This embodiment differs from Embodiment 1 in that: Step (1) copolymerization uses anionic polymerization, and the specific steps are as follows:
[0101] (1) Polymerization: Under argon atmosphere, anhydrous toluene (13 mL), i-BuAl(BHT) and 1.9(5mL, 1.6mmol, 8equiv.) aluminum reagent, initiator sec-butyl lithium (0.15mL, 0.2mmol, 1equiv.) and β-farnesene added in an amount of (4mL, 14mmol, 1400equiv.), β-myrcene (0.26mL, 1.56mmol, 156equiv.), polymerized at 25°C for 30min, and then terminated with 25mL of a mixed solution of methanol and hydrochloric acid (MeOH / HCl volume ratio = 50 / 1) and 1mL of an antioxidant. After pouring off the clear liquid, the polymer was washed three times with ethanol, and the obtained polymer was placed at 40°C and vacuum dried to constant weight to obtain an elastomeric polymer. The other steps and parameters are the same as those in Example 1.
[0102] Example 9: This example is different from Example 1 in that the hydrogenation reaction system in step (2) is replaced with a di-titaniumocene / alkyl aluminum / lithium metal compound hydrogenation system, and the specific steps are as follows:
[0103] (2) Hydrogenation: A xylene mother solution (10 wt%) of the copolymer was prepared in a 100 mL Schlenk tube. The hydrogenation reactor was dried and heated to 70° C., and 50.0 mL of the xylene mother solution (10 wt%) of the copolymer, a catalyst of dichlorotantalum (2 mg, 8 μmol, 1 equiv.), and a co-catalyst of aluminum chloride (3.2 mg, 24 μmol, 3 equiv.), and lithium hydroxide (0.96 mg, 40 μmol, 5 equiv.) were added under an argon atmosphere. The gas was replaced with H2 three times, and the pressure in the hydrogenation reactor was set to 2.5 MPa. Stirring was started, the hydrogenation reaction temperature was 60° C., the hydrogenation reaction time was 1 h, and the rotation speed was 500 rpm. After the reaction was completed, the hydrogenation reactor was cooled to room temperature, and after the pressure was released, the reactor was opened for 30.0 min, and anhydrous ethanol was added for post-treatment to obtain a white elastomer. The other steps and parameters were the same as those in Example 1.
[0104] Table 1 Data parameters of hydrogenated bio-based terpene binary random copolymer elastomer
[0105]
[0106] The above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A hydrogenated bio-based terpene binary random copolymer elastomer, characterized in that: The elastomer is prepared by copolymerization and hydrogenation of bio-based monoterpene and bio-based sesquiterpene, wherein the molar content of monoterpene polymerization unit is 5-95%, the molar content of sesquiterpene polymerization unit is 5-95%, the degree of hydrogenation is 90-99.9%, the number average molecular weight is 10,000-500,000 g / mol, and the molecular weight distribution is 1.0-5.
0.
2. The elastic body according to claim 1, characterized in that The monoterpene is one or more of geraniol, limonene, α-myrcene, β-myrcene, β-citronellol, citral, and menthol, and the sesquiterpene is one or more of cadinene, α-farnesene, β-farnesene, cedrene, and caryophyllene.
3. The elastic body according to claim 2, characterized in that The monoterpene is β-myrcene and the sesquiterpene is β-farnesene.
4. The elastic body according to claim 1, characterized in that The molar content of monoterpene polymerization units in the elastomer is 10-90%, the molar content of sesquiterpene polymerization units is 10-90%, the hydrogenation degree is 96-99%, and the molecular weight distribution is 1.9-3.
1.
5. The elastic body according to claim 1, characterized in that The glass transition temperature range of the elastomer is -80 to -50°C.
6. The elastic body according to claim 5, characterized in that The glass transition temperature of the elastomer ranges from -69 to -60°C.
7. The elastic body according to claim 1, characterized in that Elongation at break of elastomer>800%, volume resistivity>0.6×10 18 Ω.cm, melt index is 65-85g / 10min, light transmittance at 380-1100nm is 85-99%, water vapor transmission is 2-3.9%, low temperature notched impact strength at -30℃ is 50-70KJ / m 2 , cantilever beam notch impact strength is 10~20KJ / m 2 , the heat deformation temperature is 130~160℃.
8. The elastic body according to claim 7, characterized in that Elongation at break of elastomer>850%, volume resistivity>0.78×10 18 Ω.cm, melt index is 69-76g / 10min, light transmittance at 380-1100nm is 89-94%, water vapor transmission is 2.5-3.1%, low temperature notched impact strength at -30℃ is 59-65KJ / m 2 , cantilever beam notch impact strength is 13.7~15.1KJ / m 2 , the heat deformation temperature is 139~151℃.
9. The method for preparing the hydrogenated bio-based terpene binary random copolymer elastomer according to any one of claims 1 to 8, characterized in that: The method: (1) preparing a binary random copolymer by copolymerizing bio-based monoterpene and bio-based sesquiterpene monomers; (2) The binary random copolymer is dissolved in a solvent to obtain a copolymer solution, and then hydrogenated using a Ziegler-Natta hydrogenation reaction system or a metallocene hydrogenation reaction system to obtain a hydrogenated bio-based terpene binary random copolymer elastomer.
10. The method according to claim 9, characterized in that The copolymerization in step (1) adopts anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization.
11. The method according to claim 10, characterized in that The specific process of anionic polymerization is as follows: The copolymerization is initiated under anhydrous and oxygen-free conditions with an organic alkali metal as an initiator and / or an organic aluminum compound as a co-catalyst.
12. The method according to claim 11, characterized in that The organic alkali metal is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, methyllithium, ethyllithium, n-propyllithium, isopropyllithium, phenyllithium, benzyllithium, and naphthalenelithium; the organic aluminum compound can be abbreviated as AB, wherein A represents one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, and sesquiethylaluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, 2,6-di-tert-butylphenol, 2-tert-butylphenol, and 2,6-di-tert-butyl-4-ethylphenol; the reaction temperature is -50°C to 70°C, and the reaction time is 10 to 360 min.
13. The method according to claim 10, characterized in that Coordination polymerization methods include iron coordination polymerization, Zignata-type catalytic system polymerization, cationic lutetium coordination complex polymerization with β-diaminosulfonate as ligand, rare earth lanthanum catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, half-sandwich scandium complex polymerization, and cobalt catalytic system polymerization.
14. The method according to claim 13, characterized in that The specific process of using iron coordination polymerization method: Under anhydrous and oxygen-free conditions, an iron catalyst, a co-catalyst, bio-based monoterpene and bio-based sesquiterpene monomers and a solvent are added into a reactor, and a polymerization reaction is carried out at 0 to 100° C. with stirring for 10 to 120 minutes.
15. The method according to claim 14, characterized in that The iron catalyst is any one of the following structural formulas:
16. The method according to claim 9, characterized in that The concentration of the copolymer solution in step (2) is 10 wt %, and the solvent of the copolymer solution is one or more of toluene, xylene, n-hexane, and cyclohexane.
17. The method according to claim 9, characterized in that The Ziegler-Natta hydrogenation reaction process in step (2) is: Under an argon atmosphere, add a mixed liquid of the copolymer solution, the catalyst and the co-catalyst into a dry high-temperature reactor, replace the gas in the reactor three times with hydrogen, adjust the reactor speed to 200-600 rpm, the hydrogenation reaction pressure to 1-4 MPa, increase the temperature to 45-70°C, and react for 1-3 hours.
18. The method according to claim 17, characterized in that The catalyst is one or more of titanium dioxide, titanium sulfate, titanium hydroxide, nickel cyclohexaneate, nickel bromide, nickel cobalt, and nickel fluoride; the cocatalyst is an organic metal compound of metals from Group IA to Group IIIA; the mass ratio of the copolymer to the catalyst in the copolymer solution is (1-300):1; and the molar ratio of the catalyst to the cocatalyst is 1:(1-10).
19. The method according to claim 18, characterized in that The catalyst is titanium sulfate or nickel naphthenate, and the co-catalyst is one or more of aluminum acetate, aluminum hydroxide, sesquiethylaluminum chloride, DMAO and MMAO.
20. The method according to claim 9, characterized in that The metallocene hydrogenation reaction system in step (2) includes a bis(titaniacin) / lithium hydride / aromatic ester system, a bis(titaniacin) or mono(titaniacin) / triphenyllithium system, a bis(titaniacin) / alkylaluminum / silicate system or a bis(titaniacin) / alkylaluminum / lithium metal compound system.
21. The method according to claim 20, characterized in that The specific process of hydrogenation using the di-titanium / alkyl aluminum / lithium metal compound system is as follows: Under an argon atmosphere, the copolymer solution and the diocene titanocene / alkyl aluminum / lithium metal compound composite catalyst were added in sequence to a dry high-temperature reactor. The gas in the reactor was replaced three times with hydrogen. The speed of the reactor was adjusted to 200-800 rpm, the hydrogenation reaction pressure was 2.5-3.0 MPa, the temperature was increased to 50-80°C, and the reaction was carried out for 0.1-1.5 hours.
22. The method according to claim 21, characterized in that The catalyst bis-titanocenes include dichlorobis-titanocenes; the co-catalyst alkylaluminum is one or more of aluminum chloride, diethylaluminum chloride, tri-n-hexylaluminum, dimethylaluminum chloride, trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, and diisobutylaluminum hydride; the lithium-based metal compound is one or more of lithium fluoride, lithium carbonate, lithium phosphate, lithium nitride, lithium hydroxide, and lithium chloride; the mass ratio of the copolymer and the bis-titanocenes in the copolymer solution is (1-5000):1, the molar ratio of the bis-titanocenes and the alkylaluminum is 1:(1-6), and the molar ratio of the bis-titanocenes and the lithium-based metal compound is 1:(1-8).
23. The hydrogenated bio-based terpene binary random copolymer elastomer according to any one of claims 1 to 8 is used to prepare hot melt adhesives and film products thereof for use in photovoltaic solar energy and batteries, automotive interiors, clothing, footwear, electronics, wall coverings, construction, filtration or medicine.
Citation Information
Patent Citations
High-molecular-weight iron-based bio-based rubber, preparation method and application thereof, and rubber composition based on high-molecular-weight iron-based bio-based rubber
CN115073666A
Myrene / farnesene copolymer as well as preparation method and application thereof
CN118027291A
Hydrogenated terpene-polyphenol copolymer resin and adhesive composition containing said copolymer resin