Double-damping temperature range polyurethane material and preparation method thereof
By optimizing the composition and curing process of material A and material B of polyurethane materials, the problem that existing materials are difficult to take into account both low temperature and high temperature damping performance, and achieve excellent damping performance and low-cost large-scale production at low temperature and high temperature. Vibration and noise reduction in areas near automobile engines in plateau areas.
Patent Information
- Application Number
- CN202411330970.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-24
AI Technical Summary
Existing damping materials are difficult to take into account the damping performance in low-temperature and high-temperature environments at the same time, and cannot meet the vibration and noise requirements in areas near automobile engines in plateau areas.
A double-damping temperature-domain polyurethane material was designed to optimize the composition of materials A and materials B and the mixed curing process to ensure that the materials have good damping performance at low and high temperatures, including the use of polydiols and triols. The chain agent and isocyanate and other raw materials control the R value and hydroxyl molar ratio to form a suitable crosslinking network.
It achieves excellent damping performance of polyurethane materials at low and high temperatures, reduces production costs, is suitable for large-scale industrial production, and broadens the use temperature range of materials.
Smart Images

Figure CN119060296A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a double-damping temperature range polyurethane material and a preparation method thereof, belonging to the technical field of polyurethane preparation. The double-damping temperature range polyurethane material refers to a polyurethane material with good low-temperature damping performance and high-temperature damping performance. Background Art
[0002] With the continuous advancement of urbanization and industrialization, the noise and vibration pollution problems in cities and industrial areas are becoming increasingly prominent. Highways, airports, factories, construction sites, etc. are the main sources of noise and vibration. The research and development of vibration and noise reduction materials can effectively reduce the spread and impact range of noise and vibration, and improve the environmental quality of cities and industrial areas. Polyurethane is known as the "fifth largest plastic" because of its excellent mechanical properties, good deformation ability, strong biocompatibility and solvent resistance, and diverse application range. At the same time, polyurethane materials have excellent vibration and noise reduction capabilities, which can effectively absorb vibration and reduce noise. However, in response to the current problem of strong vibration and high noise in the vicinity of engines of cars, airplanes, etc. in plateau areas, the widely used material is rubber shock pads. The effective damping temperature range of such shock pads is often between -50℃ and -20℃. After starting such cars in plateau areas, the temperature in the vicinity of the engine will quickly rise from low temperature to high temperature. Therefore, the damping material here mainly requires the low-temperature and high-temperature damping properties of the material, which is difficult for existing damping and shock-absorbing materials to take into account at the same time. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide a dual-damping temperature range polyurethane material and a preparation method thereof. By improving and innovating the basic formula, a polyurethane material containing a dual damping temperature range is designed and prepared. Compared with conventional formulas, the designed formula not only has the damping performance in high and low temperature environments, but also can meet the needs of industrial mass production. This method can realize a polyurethane damping material covering both the low-temperature damping area and the high-temperature damping area at a low cost.
[0004] To achieve the above objectives, the technical solution of the present invention is as follows.
[0005] A double damping temperature range polyurethane material, which is obtained by mixing and curing material A and material B;
[0006] Taking the total mass of raw materials for preparing the A material as 100%, the components and mass fractions of each raw material are as follows:
[0007] Polyglycol 80%~90%
[0008] Triol chain extender 10%~20%
[0009] Taking the total mass of raw materials for preparing the B material as 100%, the components and mass fractions of each raw material are as follows:
[0010] Isocyanate 45%~55%
[0011] Triol or polytriol 45%~55%
[0012] The R value of B material is 4-8;
[0013] Preferably, the polyglycol in material A is at least one of polypropylene glycol (PPG), polybutylene glycol (PTMG), and polyethylene glycol (PEG), and the molecular weight of the polyglycol is 960-1200;
[0014] Preferably, the triol chain extender in material A is at least one of trimethylolpropane (TMP), triethanolamine (TEA), and glycerol (GLY);
[0015] Preferably, the isocyanate in material B is at least one of diphenylmethane diisocyanate (MDI), toluene diisocyanate (HDI) and isophorone diisocyanate (IPDI);
[0016] Preferably, the triol or polytriol in material B is at least one of polycaprolactone triol, castor oil, and polyoxypropylene triol, and the molecular weight of the triol or polytriol is 900-1100;
[0017] Preferably, the molar ratio R' of isocyanate in material B to hydroxyl in material A is 1-1.1:1, and the hydroxyl in material A refers to the sum of the number of hydroxyl groups of the polyglycol and triol chain extenders;
[0018] Preferably, the mass ratio of the triol or polytriol in the B material to the triol chain extender in the A material is 3-7:1.
[0019] A method for preparing a dual-damping temperature range polyurethane material, comprising the steps of:
[0020] (1) under the protection of protective gas, the isocyanate in material B is mixed with triol or polytriol to carry out a prepolymerization reaction to obtain a prepolymerization product, namely material B;
[0021] (2) mixing the polyglycol and the triol chain extender to obtain material A;
[0022] (3) preheating the material B and the material A at 45 to 50° C. and mixing them under air-tight conditions, and curing them to obtain the polyurethane material;
[0023] Preferably, in step (1), the prepolymerization temperature is 80-85° C. and the prepolymerization time is 4-8 h;
[0024] Preferably, in step (3), the curing temperature is 70-90° C. and the curing time is 4-8 hours.
[0025] Preferably, in the step (1), the isocyanate content in the material B is calculated by titration: the material B is added to a di-n-butylamine-toluene solution, heated and stirred at 45 to 55° C. to obtain a titration sample solution, isopropanol is added, an indicator is dripped in, and dilute hydrochloric acid is used for titration to obtain the isocyanate content;
[0026] The preparation method of the indicator is as follows: dissolving bromocresol green in a sodium hydroxide solution to obtain the indicator, wherein the ratio of the mass of bromocresol green to the volume of the sodium hydroxide solution in the indicator is 1 g:1000 mL;
[0027] The concentration of the sodium hydroxide solution is 0.1 mol / L;
[0028] The usage ratio of the indicator to the titration sample solution is 1 g:1000 mL.
[0029] The concentration of the di-n-butylamine toluene solution is 0.05-0.2 mol / L, and the usage ratio of material B to the di-n-butylamine-toluene solution is: 3 g; 70-150 mL;
[0030] The volume ratio of the titration sample solution to isopropanol is 1:2;
[0031] Preferably, the concentration of the dilute hydrochloric acid is 0.05-0.2 mol / L.
[0032] Preferably, the mass relationship between the polydiol and triol chain extender in the B material and the A material satisfies the formula:
[0033] (m1×a%) / 42=R'×((m2 / N1)×2+(m3 / N2)×3)
[0034] In the formula, m1, m2, and m3 are the masses of the polydiol and triol chain extender in material B and material A, respectively; N1 and N2 are the molecular weights of the polydiol and triol chain extender in material A, respectively; and a% is the mass fraction of isocyanate in material B obtained by titration.
[0035] Beneficial Effects
[0036] The present invention provides a dual-damping temperature range polyurethane material. The polyurethane material is a new type of polyurethane damping material, which not only has a higher loss factor, but also can meet the use requirements of damping materials under both low and high temperature working conditions. The most important point is that the synthesis cost of the material is low and can be mass-produced.
[0037] The invention provides a dual damping temperature range polyurethane material, wherein the polyurethane material is obtained by mixing and curing two components A and B according to a certain R value (ratio of isocyanate group to hydroxyl group in the material), and the selection and dosage of each substance in the A and B materials can ensure that there is a perfect and neat cross-linked network in the prepared polyurethane material, wherein the -NCO-terminated polyurethane prepolymer prepared by the B material is formed by polymerization with a triol with a larger volume, and its free volume is large, and the chain segments of this part are easy to move, so that the material can produce a glass transition at low temperature, thereby providing damping performance at low temperature, and the introduction of the triol chain extender in the A material can make the prepared polyurethane material densely distributed with small cross-linked frameworks, and these small cross-linked frameworks are not easy to move, and the chain segments can only be moved in a high temperature environment. The synergistic effect of the two can make the prepared polyurethane material have damping performance at both low and high temperatures.
[0038] The present invention provides a dual-damping temperature range polyurethane material. It is necessary to control the ratio of the triol or polytriol component of the B material to the triol chain extender component of the A material in the AB mixture. If the ratio is too high or too low, the damping temperature range of the material will only appear in the high temperature area. Only when this ratio is appropriate, a regular double cross-linked network will appear in the material, and two glass transition temperatures will be generated, so that the damping temperature range of the material is changed from high temperature to both high temperature and low temperature areas.
[0039] The present invention provides a dual-damping temperature range polyurethane material. In the preparation of the polyurethane material, both ends of the isocyanate in the B component raw material composition contain -NCO groups, and both ends of the polyol contain -OH groups. After the preliminary synthesis of the prepolymer, the two can be stored for a long time at room temperature. Subsequently, different types of polymer long chain segments (such as PTMG, PPG, etc.) and chain extension cross-linking agents (such as TMP, GLY, etc.) in the A component raw material can be added according to different production needs. The above raw materials can be polymerized at room temperature to produce polyurethane materials, and then finished products with different effects can be obtained by adjusting the ratio of A and B materials; the method is simple in steps, and the experimental formula can be changed according to production needs, and industrial production can be carried out.
[0040] The present invention provides a dual-damping temperature range polyurethane material. In the preparation of the polyurethane material, the preheating temperature of the prepolymer needs to be maintained at 45-50°C, which is the key to preserving the prepolymer. The prepolymer will self-polymerize at a temperature of 55-80°C. Both ends of the prepolymer are capped with isocyanate (-NCO) and have a tendency to polymerize with hydroxyl groups in components such as chain extenders and crosslinking agents in the main raw materials at room temperature. This polymerization method can promote the forward reaction and accelerate the reaction rate.
[0041] The invention provides a dual-damping temperature range polyurethane material. In the preparation of the polyurethane material, it is necessary to control the isocyanate content of the prepolymer. If the isocyanate content is too low, the viscosity of the polyurethane will increase, the chain will not be easy to extend, the structure will be difficult to shape, and polyurethane that can be used in practice cannot be obtained; if the isocyanate content is too high, the reaction activity will increase sharply, and it will be difficult to regulate the molding and processing of the polyurethane. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 The loss factor-temperature curves of the polyurethane materials in Examples 1 to 3 and Comparative Examples 1 to 2 are shown. DETAILED DESCRIPTION
[0043] The present invention will be further described in detail below in conjunction with specific embodiments.
[0044] Example 1
[0045] In this embodiment, the molecular weight of castor oil is 960, and the molecular weight of polypropylene glycol is 1000. The mass ratio of castor oil to trimethylolpropane is 3.93:1.
[0046] (1) 62 g of diphenylmethane diisocyanate and 36 g of castor oil were added to a 250 mL three-necked flask, the temperature was raised to 80° C. in a nitrogen environment, and the raw materials were stirred at a rate of 200 r / min to mix them evenly. After reacting for 4 h, a polyurethane prepolymer, i.e., material B, was obtained.
[0047] (2) 0.3856 g of material B obtained in step (1) was dissolved in 25 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 20 min to fully dissolve it, and 50 mL of isopropanol was added to dilute it, and then 4 drops of an indicator were added; titration was performed using 0.1023 mol / L of dilute hydrochloric acid to obtain an isocyanate content of 12.58% in the prepolymer;
[0048] (3) Preheating the prepolymer titrated in step (2) to 50° C., and preheating the main raw materials polypropylene glycol and trimethylolpropane after dehydration to 50° C.
[0049] (4) Add 16.00 g of polypropylene glycol and 3.00 g of trimethylolpropane in step (3) into a container in sequence, then add 31.00 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 20 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70° C. for curing for 4 hours to obtain a dual-damping temperature range polyurethane material.
[0050] Example 2
[0051] In this embodiment, the molecular weight of polycaprolactone triol is 1000, and the molecular weight of polybutylene glycol is 1000. The ratio of polycaprolactone triol to triethanolamine is 5.19:1.
[0052] (1) 50 g of isophorone diisocyanate and 50 g of polycaprolactone triol were added to a 250 mL three-necked flask, the temperature was raised to 80° C. in a nitrogen environment, and the raw materials were stirred at a rate of 200 r / min to mix them evenly. After reacting for 4 h, a polyurethane prepolymer was obtained.
[0053] (2) 0.3841 g of the prepolymer obtained in step (1) was dissolved in 25 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 20 min to fully dissolve it, and 50 mL of isopropanol was added for dilution, and then 4 drops of bromocresol green indicator were added; titration was performed using 0.1023 mol / L of dilute hydrochloric acid to obtain an isocyanate content of 12.35% in the prepolymer;
[0054] (3) Preheating the prepolymer titrated in step (2) to 50° C., and preheating the main raw materials polybutylene glycol and triethanolamine after dehydration to 50° C.
[0055] (4) Add 16.30 g of polybutylene glycol and 2.96 g of triethanolamine in step (3) into a container in sequence, then add 30.74 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 20 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70° C. for curing for 4 hours to obtain a dual-damping temperature range polyurethane material.
[0056] Example 3
[0057] In this embodiment, the molecular weight of polyoxypropylene is 1080, and the molecular weight of polyethylene glycol is 1000. The mass ratio of polyoxypropylene to glycerol is 4.81:1.
[0058] (1) 55 g of toluene diisocyanate and 45 g of polyoxypropylene were added to a 250 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly. After reacting for 4 h, a polyurethane prepolymer was obtained.
[0059] (2) 0.3526 g of the prepolymer obtained in step (1) was dissolved in 25 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 20 min to fully dissolve it, and 50 mL of isopropanol was added for dilution, and then 4 drops of bromocresol green indicator were added; titration was performed using 0.1023 mol / L of dilute hydrochloric acid to obtain an isocyanate content of 12.53% in the prepolymer;
[0060] (3) Preheating the prepolymer titrated in step (2) to 50° C., and preheating the main raw materials polyethylene glycol and glycerol after dehydration to 50° C.
[0061] (4) Add 16.43 g of polyethylene glycol and 2.87 g of glycerol in step (3) into a container in sequence, then add 30.70 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 20 seconds; pour the solution into a polytetrafluoroethylene container and place it in an oven at 70° C. for curing for 4 hours to obtain a dual-damping temperature range polyurethane material.
[0062] Comparative Example 1
[0063] In this comparative example, the molecular weight of castor oil is 960, and the molecular weight of polypropylene glycol is 900. This comparative example uses the same material B as Example 1, but the material A does not contain a small molecule cross-linking agent, but a diol chain extender is used instead.
[0064] Steps (1)-(2) are the same as in Example 1,
[0065] (3) Preheating the prepolymer titrated in step (2) to 50° C., and preheating the main raw materials polypropylene glycol and 1,4-butanediol after dehydration to 50° C.
[0066] (4) Add 22.32 g of polypropylene glycol and 2 g of 1,4-butanediol in step (3) into a container in sequence, then add 25.68 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 20 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70° C. for curing for 4 hours to obtain a polyurethane material.
[0067] Comparative Example 2
[0068] The molecular weight of the polypropylene glycol in this comparative example is 1000. In this comparative example, no triol or polytriol is added to the prepolymer, that is, the prepolymer is a linear system, and the mass ratio of the macromolecular diol to the crosslinking agent in material A is the same as that in Example 1.
[0069] Steps (1)-(2) are the same as in Example 1,
[0070] (3) Preheating the prepolymer titrated in step (2) to 50° C., and preheating the main raw materials polypropylene glycol and trimethylolpropane after dehydration to 50° C.
[0071] (4) Add 15.29 g of polypropylene glycol and 2.87 g of trimethylolpropane in step (3) into a container in sequence, then add 31.85 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 20 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70° C. for curing for 4 hours to obtain a polyurethane material.
[0072] The final products prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to DMA test. The test conditions were tensile mode, and a 30 mm × 5 mm × 2 mm strip sample was used for fixed frequency variable temperature test at 10 Hz. The test temperature range was -100°C to 100°C. The results are shown in FIG. Figure 1 As shown, Examples 1 to 3 show loss factor peak shapes and phenomena that are significantly different from those of Comparative Examples 1 and 2. Comparative Examples 1 and 2 are samples prepared using cross-linked material B and material A containing a cross-linking chain extender, respectively, while Examples 1 to 3 use both cross-linked material B and introduce a small molecule cross-linking agent into material A to form a double cross-linked network. Not only is the loss factor in the high temperature region close to that of Comparative Examples 1 to 2, but there is also a trend of moving to a higher temperature. Moreover, Examples 1 to 3 with a double cross-linked network also produce a damping temperature range in the low temperature region, broadening the use temperature range of polyurethane materials as damping materials. At the same time, the damping temperature range of the material can be adjusted by changing the diol and isocyanate components used in the matrix. Targeted design is achieved.
[0073] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. A dual damping temperature range polyurethane material, characterized in that: The polyurethane material is obtained by mixing and curing material A and material B; Taking the total mass of raw materials for preparing material A as 100%, the composition and mass fraction of each raw material are as follows: Polyglycol 80%~90% Triol chain extender 10%~20% Taking the total mass of raw materials for preparing material B as 100%, the components and mass fractions of each raw material are as follows: Isocyanate 45%~55% Triol or polytriol 45% to 55%.
2. A dual damping temperature range polyurethane material according to claim 1, characterized in that: The R value of the B material is 4-8.
3. A dual damping temperature range polyurethane material according to claim 1 or 2, characterized in that: In the material A, the polyglycol is at least one of polypropylene glycol, polybutylene glycol and polyethylene glycol, and the molecular weight of the polyglycol is 960-1200; In the material A, the triol chain extender is at least one of trimethylolpropane, triethanolamine and glycerol.
4. A dual damping temperature range polyurethane material according to claim 3, characterized in that: In the material B, the isocyanate is at least one of diphenylmethane diisocyanate, toluene diisocyanate, and isophorone diisocyanate; In the material B, the triol or polytriol is at least one of polycaprolactone triol, castor oil, and polyoxypropylene triol, and the molecular weight of the triol or polytriol is 900-1100; In the material B, the molar ratio R' of isocyanate to hydroxyl in the material A is 1-1.1:1; The hydroxyl group in material A refers to the sum of the hydroxyl groups of the polydiol and triol chain extenders; In the B material, the mass ratio of the triol or polytriol to the triol chain extender in the A material is 3-7:
1.
5. A method for preparing a dual-damping temperature range polyurethane material, characterized in that The steps include: (1) Under the protection of protective gas, isocyanate is mixed with triol or polytriol to carry out prepolymerization reaction to obtain material B; (2) mixing the polyglycol and the triol chain extender to obtain material A; (3) In an airtight condition, preheat the material B and the material A at 45-50° C. and mix them, and obtain a dual-damping temperature range polyurethane material after curing.
6. The method for preparing a dual-damping temperature range polyurethane material according to claim 5, characterized in that: In the step (1), the prepolymerization temperature is 80-85° C. and the prepolymerization time is 4-8 hours.
7. The method for preparing a dual-damping temperature range polyurethane material according to claim 5, characterized in that: In the step (3), the curing temperature is 70-90° C. and the curing time is 4-8 hours.
8. The method for preparing a dual-damping temperature range polyurethane material according to claim 5, characterized in that: In the step (1), the content of isocyanate in the obtained material B is calculated by titration, the steps are: Add the obtained material B to a toluene solution of di-n-butylamine, and heat and stir at a temperature of 45-55° C. to obtain a titration sample solution; Isopropanol is added to the titration sample solution, and then the indicator is dropped in, and dilute hydrochloric acid is used for titration to obtain the isocyanate content.
9. The method for preparing a dual-damping temperature range polyurethane material according to claim 8, characterized in that: The preparation method of the indicator is as follows: dissolving bromocresol green in a sodium hydroxide solution to obtain the indicator, wherein the ratio of the mass of bromocresol green to the volume of the sodium hydroxide solution in the indicator is 1 g:1000 mL; The sodium hydroxide concentration is 0.1 mol / L; The usage ratio of the indicator to the titration sample solution is 1 g:1000 mL.
10. The method for preparing a dual-damping temperature range polyurethane material according to claim 8, characterized in that: The concentration of the di-n-butylamine toluene solution is 0.05-0.2 mol / L, and the dosage ratio of material B to the di-n-butylamine toluene solution is: 3g: 70-150mL; The volume ratio of the titration sample solution to isopropanol is 1:2; The concentration of the dilute hydrochloric acid is 0.05-0.2 mol / L; The mass relationship between the polydiol and triol chain extender in the B material and the A material satisfies the formula: (m1×a%) / 42=R'×((m2 / N1)×2+(m3 / N2)×3) In the formula, m1, m2, and m3 are the masses of the polydiol and triol chain extender in material B and material A, respectively; N1 and N2 are the molecular weights of the polydiol and triol chain extender in material A, respectively; and a% is the mass fraction of isocyanate in material B obtained by titration.
Citation Information
Patent Citations
Preparation method for polyurethane damping material containing suspension chain structure
CN101220132A
Hindered phenol dangled polyurethane damping material and preparation method thereof
CN102898606A
High-performance polyurethane damping material containing dynamic disulfide bonds and preparation method thereof
CN116554430A
Laminated damping type polyurethane elastomer and preparation method thereof
CN118404880A
Low-damping polyurethane elastomer
US20190276582A1
Cited By
Vibrating diaphragm for sound production device, sound production device and electronic equipment
CN120602852A
Wide-temperature-range polyurethane material with excellent adhesive property and preparation method of wide-temperature-range polyurethane material
CN120923715A