Method for preparing electrocatalyst based on metal organic framework (MOF) and method for preparing dissolved oxygen saturated solution by using electrocatalyst

Through the preparation and application of CoFe0.2-MOF material, the problems of rare metal electrocatalyst reserves and inaccurate preparation of dissolved oxygen solutions are solved, and high-efficiency electrolytic aquatic oxygen and accurate dissolved oxygen detection are achieved, reducing costs and improving electrocatalytic performance .

CN119060346APending Publication Date: 2024-12-03AIMOLI (HEBEI) TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411091480.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing precious metal electrocatalysts have few reserves and high prices on the earth, as well as the lack of efficient non-precious metal electrocatalysts and accurate preparation methods for dissolved oxygen saturated solutions, limiting the efficiency of electrolytic aquatic oxygen production and the accuracy of dissolved oxygen detection.

Method used

CoFe0.2-MOF material is used as an electrocatalyst, and the electrocatalyst is prepared by FeCl3·6H2O and Co(NO3)2·6H2O in N,N-dimethylacetamide solution, combined with hydrothermal reaction, and sodium nitrite is used to synthesize the electrocatalyst. Adjust the dissolved oxygen content to prepare saturated dissolved oxygen solution in batches.

Benefits of technology

The electrocatalytic performance with low overpotential and Tafel slope is achieved, the oxygen efficiency of electrolytic aquatic production is improved, and the accurate dissolved oxygen saturated solution is prepared quickly and conveniently, reducing the use demand of precious metal electrocatalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004986698400000011
    Figure HDA0004986698400000011
  • Figure HDA0004986698400000021
    Figure HDA0004986698400000021
  • Figure HDA0004986698400000031
    Figure HDA0004986698400000031
Patent Text Reader

Abstract

The invention relates to the field of hydrogen evolution and oxygen evolution reaction of electrolyzed water, and provides preparation of an MOF (Metal Organic Framework) material taking Co and Fe ions as metal ions and a method for preparing a dissolved oxygen saturated solution by using the MOF material. The preparation method comprises the following steps: firstly, dissolving Co (NO3) 2.6 H2O and FeCl3. 6H2O in a N, N-dimethylacetamide (DMA) solution, after fully dissolving, adding terephthalic acid (1, 4-BDC) as an organic linker, and after uniformly dispersing, adding 1, 4-diazabicyclo [2.2. 2] octane (dabco) as a regulator; secondly, putting the obtained suspension into a hydrothermal kettle for hydrothermal reaction, adding the obtained dark green solid into a centrifugal tube, and respectively washing with absolute ethyl alcohol and deionized water for three times and two times; and finally, putting the solid in the centrifugal tube into a drying oven, and carrying out drying treatment to obtain a faint yellow solid substance. The electrocatalyst prepared by the method provided by the invention has very low overpotential and Tafel slope, can efficiently electrolyze water to produce hydrogen and oxygen, and prepares a dissolved oxygen saturated solution for a calibration device of an optical dissolved oxygen sensor based on oxygen production of an anode during electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrocatalytic hydrogen and oxygen evolution, and in particular to a method for preparing an electrocatalyst designed with MOF materials and applying the electrocatalyst to prepare a dissolved oxygen saturated solution. Background Art

[0002] To improve the efficiency of hydrogen and oxygen production by water electrolysis, the core technology is to improve the catalytic performance of electrocatalysts and reduce overpotential and Tafel slope. For commercial water electrolysis materials, the electrocatalysts used on the anode are generally ruthenium dioxide (RuO2) and iridium dioxide (IrO2), and the electrocatalysts used on the cathode are generally platinum carbon alloy (Pt / C). These precious metal electrocatalysts have very low overpotential and Tafel slope. However, the scarce reserves of these precious metals on the earth and the high prices limit the large-scale commercial application of these precious metal electrocatalysts. Therefore, it is necessary to develop a low-cost and efficient non-precious metal electrocatalyst. At present, the most studied non-precious metal electrocatalysts are Ni, Fe, and Co-based electrocatalysts. These non-precious metal electrocatalysts have very low overpotential and Tafel slope, and some have extremely high stability. For OER reactions, the performance of some electrocatalysts is even better than that of commercial RuO2.

[0003] MOF materials are popular materials developed in recent years. They have the advantages of adjustable pores and high specific surface area. They have been studied and applied in many fields such as gas adsorption, ion exchange, and heterogeneous catalysis. Due to the advantages of MOF materials themselves, they will also have potential value in the field of electrocatalysis. Currently, Ni-based MOF materials are widely explored, and most of the research on Co-based MOF materials is still vacant. In general MOF synthesis methods, DMF is used as the solvent, and other solutions are rarely explored as solvents.

[0004] The amount of dissolved oxygen in water is an indicator of the self-purification ability of water bodies and is also an indispensable living condition for aquatic organisms. Therefore, the determination of dissolved oxygen is of great significance in sewage treatment, medical diagnosis, water source detection and research. Currently, sensor detection has become increasingly mature and has been widely used.

[0005] The premise for ensuring data accuracy of optical and electrochemical dissolved oxygen sensors is sensor calibration. Only after calibration can the sensor output the corresponding dissolved oxygen value. The calibration method proposed in the "National Environmental Protection Standard of the People's Republic of China HJ506-2009" is two-point calibration, namely zero-point calibration and saturated oxygen calibration. The standard only mentions possible saturation, but does not tell the method and conditions required to achieve saturation. Currently, commercially available dissolved oxygen sensors are calibrated at two points (zero point, saturated oxygen) or one point (saturated oxygen) before leaving the factory, because it is generally believed that the zero point will not drift over time, so some manufacturers use one-point calibration. Regardless of the calibration method, a saturated oxygen solution is required. Therefore, the accuracy of the saturated solution determines the accuracy of the sensor, which is of great significance to the calibration of the sensor. However, there is currently no mature and accurate method for preparing saturated dissolved oxygen solutions. Summary of the invention

[0006] In view of this, the present invention provides a method for preparing a Co, Fe bimetallic MOF material and applying it to prepare a dissolved oxygen saturated solution. The material is named CoFe0.2-MOF. The CoFe0.2-MOF electrocatalytic material provided by the present invention has a very low overpotential and a very low Tafel slope.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] A method for preparing a CoFe0.2-MOF material comprises the following steps:

[0009] N,N-dimethylacetamide (DMA) was used as the solution;

[0010] FeCl3·6H2O was used as the Fe source, and then it was added to the DMA solution with Co(NO3)2·6H2O in a certain molar ratio. Then terephthalic acid (1,4-BDC) was added as an organic linker, and finally 1,4-diazabicyclo[2.2.2]octane (dabco) was added as a regulator. The obtained suspension was subjected to hydrothermal reaction, and the obtained solid was centrifuged and dried to obtain a light yellow solid.

[0011] Preferably, the molar ratio of Co(NO3)2·6H2O and FeCl3·6H2O is (4-9):1.

[0012] Preferably, the hydrothermal temperature is 110 to 130 degrees and the time is 24 to 48 hours.

[0013] The invention provides a method for preparing a CoFe0.2-MOF material.

[0014] The general DMF solution was replaced by DMA solution.

[0015] FeCl3·6H2O is used as the Fe source, and Fe ions and Co ions are used together as metal ion ligands in the MOF material to form a bimetallic MOF material. The synergistic effect of Fe ions and Co ions will greatly promote the reaction rate in the OER process, reduce the overpotential and Tafel slope, and produce oxygen more efficiently in water electrolysis.

[0016] The present invention provides a device for preparing saturated oxygen solution, which can conveniently and quickly prepare dissolved oxygen saturated solution in batches, comprising the following steps:

[0017] A water electrolysis device was prepared using the prepared CoFe0.2-MOF electrocatalytic material;

[0018] The electrolysis time is T1;

[0019] Determine the dissolved oxygen content of the water at the anode, and calculate the sodium nitrite content required to reduce the dissolved oxygen content of the solution to be used from supersaturated to the theoretical saturated value by comparing it with the theoretical saturated dissolved oxygen value under the environment;

[0020] Sodium nitrite is added simultaneously to obtain a solution saturated with dissolved oxygen;

[0021] Effect of the present invention: dissolved oxygen saturated solution can be prepared quickly in batches. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagrams and morphology and composition characterization diagrams of CoFe0.2-MOF materials, where (a) is a schematic diagram of the sample preparation process; (b) is a SEM image of the CoFe0.2-MOF material; (c) is the morphology of CoFe0.2-MOF under HRTEM; (d) is the element distribution diagram of the CoFe0.2-MOF material under EDS scanning.

[0023] Figure 2 The electrocatalytic performance diagrams of MOF materials composed of different metal ions in Application Example 1. (a) is the linear sweep voltammetric characteristic curve (LSV); (b) is the electrochemical impedance spectroscopy (EIS).

[0024] Figure 3 The performance diagrams of the electrocatalysts obtained with different FeCl3·6H2O contents in Application Example 2. (a) is the linear sweep voltammetric characteristic curve (LSV); (b) is the electrochemical impedance spectroscopy (EIS); and (c) is the fitted Tafel slope diagram.

[0025] Figure 4 The performance diagrams of the electrocatalysts obtained at different hydrothermal temperatures in Application Example 3. (a) is the linear sweep voltammetric characteristic curve (LSV); (b) is the electrochemical impedance spectroscopy (EIS); and (c) is the fitted Tafel slope diagram.

[0026] Figure 5 The performance diagrams of the electrocatalysts obtained at different hydrothermal times in Application Example 4. (a) is the linear sweep voltammetric characteristic curve (LSV); (b) is the electrochemical impedance spectroscopy (EIS); and (c) is the fitted Tafel slope diagram. DETAILED DESCRIPTION

[0027] In the present invention, all medicines are from Aladdin manufacturer. Unless otherwise specified, the deionized water used in all links comes from the laboratory's water purifier.

[0028] In the present invention, the production steps of the same batch of samples are synthesized by the same personnel, and the models of instruments such as beakers and ovens are kept consistent during the production process.

[0029] In the present invention, the rotation speed of the stirrer is preferably 400 rpm.

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] Mix 4.8mmol Co(NO3)2·6H2O with 45ml DMF solution, maintain the stirring speed at 400rpm at room temperature, and maintain this stirring speed in subsequent stirring. After stirring for five minutes, add 1.2mmol FeCl3·6H2O, stir for five minutes, add 6mmol 1,4-BDC, stir for 10 minutes, and after 1,4-BDC is fully mixed, add 3mmol dabco, cover with plastic wrap, and stir for 2h. Transfer the resulting suspension to a 100ml polytetrafluoroethylene liner for hydrothermal reaction, set the heating temperature to 120 degrees, and heat for 48h. After the reactor is naturally cooled to room temperature, rinse the obtained dark green solid material in a centrifuge tube with ethanol, centrifuge again, repeat this operation three times, and then rinse with deionized water. The operation method is the same as ethanol, but rinse twice. Finally, dry the obtained solid material in an oven at 60 degrees for 24h to obtain a light yellow solid.

[0033] The obtained samples were characterized and tested, and the obtained SEM and TEM images are shown in Figure 1 As shown, Figure 1(a) is a schematic diagram of sample preparation; (b) is a SEM image of the surface of CoFe-MOF material; (c) is the corresponding TEM image; (d) is the corresponding EDS image. Figure 1 From (d), it can be seen that the Fe element is successfully distributed inside the sample.

[0034] In addition, as a comparison, keeping other conditions unchanged, this experiment synthesized MOF materials with different metal ion compositions. Using Ni(NO3)2·6H2O as the Ni source and Co(NO3)2·6H2O as the Co source, Ni-MOF, Co-MOF, Fe-MOF, NiFe0.2-MOF, CoFe0.2-MOF, and NiCo0.2Fe0.2-MOF were synthesized respectively.

[0035] Application Example 1

[0036] This application example uses the different metal ion MOF materials synthesized in Example 1 to perform electrochemical performance testing. The specific steps are as follows:

[0037] Weigh 4 mg of the obtained solid, put it in a small glass bottle, add 750ul and 250ul of deionized water and ethanol respectively, then ultrasonically treat the solution for 30 minutes, add 50ul of Nafion solution, and ultrasonically treat it again for 30 minutes. Use a pipette to draw 5ul of the obtained solution and drop it on the polished glassy carbon electrode. The carbon core diameter of the glassy carbon electrode is 3mm. The glassy carbon electrode is placed in an oven to dry for 2 to 3 minutes. Finally, the electrochemical performance of the sample is tested using an electrochemical workstation. The saturated calomel electrode is used as the production electrode, and 1mol / L KOH is used as the dielectric of the three-electrode system. After calculation, the mass of the sample covered on the surface of the glassy carbon electrode is approximately 0.067mg.

[0038] The calculation formula of Tafel slope is shown in formula (1):

[0039] η=a+b*lg|i| (1)

[0040] In formula (1), b is the Tafel slope, η is the overpotential, and i is the current density.

[0041] The test results are as follows Figure 2 As shown, Figure 2 The results show that the overpotentials of MOF materials composed of different metal ions are 308mV, 432mV, 492mV, 369mV, 304mV, and 438mV, respectively. Among the MOF materials composed of different metal ions, CoFe-MOF material has the best electrocatalytic performance and has a very low overpotential and Tafel slope.

[0042] Application Example 2

[0043] This example uses different concentrations of FeCl3·6H2O to explore the experiment. The specific operation steps are as follows:

[0044] According to the method in Example 1, while keeping other conditions unchanged, 1.2mmol FeCl3·6H2O was replaced with 0.15mmol, 0.3mmol, 0.6mmol, 1.2mmol, and 1.8mmol FeCl3·6H2O, respectively. Finally, the electrochemical performance test of the five groups of samples obtained was carried out, and the electrochemical performance test method was consistent with the method in Application Example 1.

[0045] The test results are as follows Figure 3 As shown, it can be seen that in this embodiment, the overpotentials of the samples obtained by adding different contents of FeCl3·6H2O are 393mV, 308mV, 300mV, 306mV, 323mV, respectively, and the Tafel slopes are 69.31mV / dec, 38.69mV / dec, 41.89mV / dec, 39.67mV / dec, and 41.92mV / dec, respectively.

[0046] Application Example 3

[0047] This example uses different hydrothermal temperatures for exploration experiments. The experimental operation steps are as follows:

[0048] According to the method in Example 1, while keeping other conditions unchanged, the original hydrothermal temperature of 120 degrees was replaced with 100 degrees, 120 degrees, 140 degrees, 160 degrees, and 180 degrees respectively. Five groups of samples were obtained under the same operating conditions, and finally the electrochemical performance of the five groups of samples was tested according to the method in Application Example 1.

[0049] The test results are as follows Figure 4 As shown, Figure 4 The results show that in this embodiment, the overpotentials of the samples obtained at different hydrothermal temperatures are 331mV, 310mV, 308mV, 337mV, and 327mV, respectively, and the Tafel slopes are 38.27mV / dec, 39.59mV / dec, 41.94mV / dec, 38.49mV / dec, and 40.33mV / dec, respectively.

[0050] Application Example 4

[0051] This example uses an exploratory experiment with different hydrothermal times. The experimental operation steps are as follows:

[0052] According to the method in Example 1, while keeping other conditions unchanged, the original 48h hydrothermal time was replaced with 36h, 42h, 48h, 54h, and 60h respectively. Five groups of samples were obtained under the same operating conditions, and finally the electrochemical performance of the five groups of samples was tested according to the method in Application Example 1.

[0053] The test results are as follows Figure 5 As shown, it can be seen that in this embodiment, the overpotentials of the samples obtained at different hydrothermal times are 297 mV, 296 mV, 311 mV, 306 mV, and 303 mV, respectively, and the Tafel slopes are 37.75 mV / dec, 37.83 mV / dec, 39.24 mV / dec, 37.97 mV / dec, and 39.71 mV / dec, respectively.

Claims

1. A method for preparing a Co- or Fe-based MOF electrocatalyst material, characterized in that: The following steps are involved: FeCl3·6H2O was doped into Co-MOF material as Fe source to construct Co and Fe dual ion synergistic electrocatalytic material. Using N,N-dimethylacetamide as solvent instead of N,N-dimethylformamide as solvent, the electrocatalyst performance obtained by using N,N-dimethylacetamide as solvent is better.

2. The preparation method according to claim 1, characterized in that: The molar ratio of Co(NO3)2·6H2O and FeCl3·6H2O is (4-9):

1.

3. The preparation method according to claim 1, characterized in that: The hydrothermal temperature is 110 to 130 degrees and the time is 24 to 48 hours.

4. The preparation method according to claim 1, characterized in that: The prepared electrocatalyst was used to electrolyze water to form a saturated oxygen solution.