Antibacterial material for shoes and preparation method thereof

By modifying the chemical action of titanium dioxide and ethylene propylene ternary rubber and isothiazolinone structure, the aging and odor problems of shoe materials are solved, and efficient antibacterial and anti-ultraviolet effects are achieved, and the service life of shoe materials is extended.

CN119060460AInactive Publication Date: 2024-12-03含山县华侨鞋业有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411127312.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Shoe materials are prone to aging during use, resulting in the generation of odors and bacterial growth. The organic small molecule ultraviolet absorbers added in the prior art fail over time, affecting the service life of the shoe body material.

Method used

Modified titanium dioxide is used to form covalent bonds through chemical interaction with ethylene propylene tereum rubber, which improves its dispersion and interface compatibility, and uses isothiazolinone structure to kill bacteria and is also resistant to ultraviolet rays. Effects: An antibacterial material for shoes was prepared.

Benefits of technology

It achieves efficient and long-lasting antibacterial effects and anti-ultraviolet effects, extends the service life of the shoe body material, and prevents the generation of odors and bacterial growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004996817550000021
    Figure BDA0004996817550000021
  • Figure BDA0004996817550000022
    Figure BDA0004996817550000022
  • Figure BDA0004996817550000071
    Figure BDA0004996817550000071
Patent Text Reader

Abstract

The invention discloses an antibacterial material for shoes and a preparation method thereof, and belongs to the technical field of high polymer materials. The invention relates to an antibacterial material for shoes. The antibacterial material comprises the following raw materials in parts by weight: 70-80 parts of ethylene propylene diene monomer, 10-20 parts of polyethylene, 20-30 parts of modified titanium dioxide, 10-20 parts of a reinforcing agent, 1.5-4.5 parts of a lubricant, 1-3 parts of a vulcanizing agent, 0.5-1.5 parts of an anti-aging agent and 0.5-0.8 part of an initiator. The modified titanium dioxide contains titanium dioxide and isothiazolinone structures, and a chemical action exists between the modified titanium dioxide and the ethylene propylene diene monomer, so that the modified titanium dioxide can be highly dispersed and stably exist in the antibacterial material for the shoes and fully and stably play a role; therefore, the antibacterial material for the shoes has efficient and lasting antibacterial effect and anti-ultraviolet effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to an antibacterial material for shoes and a preparation method thereof. Background Art

[0002] Shoes are a necessity in people's daily life. With the development of science and technology and the improvement of people's living standards, people's requirements for the quality and performance of shoes are getting higher and higher.

[0003] When people walk, the sweat glands on their feet will secrete secretions, which will produce odors when decomposed by bacteria and molds, especially after heavy sweating caused by strenuous exercise. The soles of the feet have many sweat glands and are prone to sweating. In addition to water and salt, sweat also contains lactic acid and urea. Under the condition of excessive sweating, the bacteria on the feet will multiply and decompose keratin, and the urea and lactic acid in the sweat will produce a bad smell. At the same time, the growth and reproduction of bacteria can also cause athlete's foot.

[0004] In addition, shoe materials are prone to aging when exposed to direct sunlight for a long time, causing the shoes to crack and affecting their use. The prior art usually combats ultraviolet rays by adding small organic molecule ultraviolet absorbers. However, small organic molecule ultraviolet absorbers migrate and fall out of the shoe material as the use time increases, and then lose their effectiveness, ultimately greatly reducing the service life of the shoe material. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide an antibacterial material for shoes and a preparation method thereof.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] An antibacterial material for shoes comprises the following raw materials in parts by weight: 70-80 parts of EPDM rubber, 10-20 parts of polyethylene, 20-30 parts of modified titanium dioxide, 10-20 parts of reinforcing agent, 1.5-4.5 parts of lubricant, 1-3 parts of vulcanizing agent, 0.5-1.5 parts of antioxidant, and 0.5-0.8 parts of initiator.

[0008] Furthermore, the modified titanium dioxide is prepared by the following steps:

[0009] S1. A three-necked flask was dried and purged with nitrogen to drive away the air in the flask, and then 5-chloro-2-methyl-4-isothiazoline-3-one, triethylamine and DMSO (dimethyl sulfoxide) were added, stirred until completely dissolved, and then 3-butene-1-amine was slowly added. After the addition was completed, the temperature was controlled at 5°C to react for 8 hours. After the reaction was completed, it was distilled under reduced pressure, purified by column chromatography (a mixed solvent of benzene and acetone was selected as the eluent, and the volume ratio of benzene and acetone was 9:1), and distilled under reduced pressure to obtain intermediate 1; the amounts of 5-chloro-2-methyl-4-isothiazoline-3-one, 3-butene-1-amine, triethylamine and DMSO were 0.08 mol: 0.088 mol: 16 mL: 100 mL;

[0010] Triethylamine is used as an acid-binding agent, and the -Cl of 5-chloro-2-methyl-4-isothiazoline-3-one and the -NH2 of 3-butene-1-amine undergo a nucleophilic substitution reaction. The reaction process is as follows:

[0011]

[0012] S2. Under nitrogen protection, add intermediate 1, DBU (1,8-diazobisspiro[5.4.0]undec-7-ene) and DMSO into a three-necked flask, stir evenly, then slowly add coupling agent KH570 (3-(methacryloyloxy)propyltrimethoxysilane), heat to 60°C and react for 48h. After the reaction, distill under reduced pressure to obtain intermediate 2; the dosage ratio of intermediate 1, coupling agent KH570, DBU and DMSO is 0.07mol:0.075mol:2.1mL:130mL;

[0013] Under the catalytic action of DBU, intermediate 1 undergoes Michael addition reaction with coupling agent KH570. The reaction process is as follows:

[0014]

[0015] S3, titanium dioxide and deionized water are added to a three-necked flask, mixed evenly, and concentrated hydrochloric acid is added dropwise to adjust the pH value to 5, and the temperature is raised to 65°C while stirring, and the mixed solution of DMSO and intermediate 2 is slowly added to the above three-necked flask under stirring, and the mixture is kept warm and stirred for 10 hours after the addition is completed, and then cooled to room temperature, the mixture is filtered, and washed with anhydrous ethanol for 5 times. After washing, the product is vacuum dried at 80°C for 12 hours to obtain modified titanium dioxide. The mass ratio of titanium dioxide to intermediate 2 is 20:1.

[0016] The trimethoxysilane on the intermediate 2 can be hydrolyzed and then condensed to form Si-O-Si and Si-OH; the hydroxyl group in the silanol group can form a hydrogen bond with the hydroxyl group on the surface of the titanium dioxide, and then dehydrate and condense to form a covalent bond, thereby greatly reducing the surface energy of the titanium dioxide, making it uniformly dispersed in the antibacterial material. In addition, the surface of the modified titanium dioxide has an oil-soluble heterocyclic structure, ester group, etc., which further reduces the surface energy of the modified titanium dioxide and improves its dispersion. At the same time, the surface of the modified titanium dioxide contains carbon-carbon double bonds, which can react chemically with the unsaturated double bonds of the side chain of EPDM rubber under the action of an initiator, thereby further improving the interfacial compatibility of the modified titanium dioxide and the base rubber. The modified titanium dioxide is also not easy to fall off from the sole material, and can fully and stably exert its anti-ultraviolet and antibacterial effects.

[0017] Modified titanium dioxide contains isothiazolinone structure, which kills by breaking the bonds of bacterial proteins. After contacting with microorganisms, it can quickly and irreversibly inhibit their growth, thereby leading to the death of microbial cells. It has a strong inhibitory and killing effect on common bacteria, fungi, algae, etc.; the isothiazolinone structure has the characteristics of high killing efficiency, good degradability, no residue, safe operation, good compatibility, strong stability, and low cost of use.

[0018] The titanium dioxide in modified titanium dioxide can effectively fight against bacteria such as Staphylococcus aureus and Escherichia coli that cause odor in shoes, reducing odor caused by bacteria; titanium dioxide can absorb and reflect ultraviolet rays, protect materials and slow down aging.

[0019] The synergistic effect of titanium dioxide and isothiazolinone structure gives the modified titanium dioxide excellent antibacterial effect, while the modified titanium dioxide itself has excellent anti-ultraviolet effect.

[0020] Furthermore, the reinforcing agent is one or more of carbon black, nano calcium carbonate, and fumed silica.

[0021] Furthermore, the lubricant is a mixture of stearic acid and zinc stearate in a mass ratio of 1:2.

[0022] Furthermore, the vulcanizing agent is sulfur.

[0023] Furthermore, the antioxidant is one or more of antioxidant D, antioxidant SP, antioxidant AW, and antioxidant RD.

[0024] Furthermore, the initiator is di-tert-butyl peroxide.

[0025] A method for preparing an antibacterial material for shoes comprises the following steps:

[0026] Mix EPDM rubber, polyethylene, modified titanium dioxide, reinforcing agent and initiator evenly, pour into internal mixer, and mix at 100-110℃ for 10min; add lubricant and antioxidant, heat up to 120-130℃, continue mixing for 10-15min to obtain mixed rubber; finally heat up to 150-160℃, add vulcanizing agent and vulcanize for 5-8min, melt granulate after vulcanization, and compression mold to obtain antibacterial material for shoes.

[0027] Beneficial effects of the present invention: the modified titanium dioxide contains titanium dioxide and isothiazolinone structures, and there is a chemical reaction between the modified titanium dioxide and the EPDM rubber. Therefore, the modified titanium dioxide can be highly dispersed and stably present in the antibacterial material for shoes, fully and stably play its role, so that the antibacterial material for shoes of the present invention has efficient and lasting antibacterial effect and anti-ultraviolet effect. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] The specific steps for preparing modified titanium dioxide are as follows:

[0031] S1, nitrogen was blown into a 250 mL dry three-necked flask to drive away the air in the flask, and then 9.6 mL of 5-chloro-2-methyl-4-isothiazoline-3-one, 16 mL of triethylamine and 100 mL of DMSO were added, and stirred until completely dissolved, and then 6.3 g of 3-butene-1-amine was slowly added. After the addition was completed, the temperature was controlled at 5°C to react for 8 hours. After the reaction was completed, it was distilled under reduced pressure, purified by column chromatography (the eluent was a mixed solvent of benzene and acetone, and the volume ratio of benzene and acetone was 9:1), and distilled under reduced pressure to obtain intermediate 1;

[0032] S2, under nitrogen protection, add 12.9g of intermediate 1, 2.1mL of DBU and 130mL of DMSO into a 250mL three-necked flask, stir evenly, then slowly add 17.8mL of coupling agent KH570, after adding, heat to 60°C and react for 48h, after the reaction, distill under reduced pressure to obtain intermediate 2;

[0033] S3. Add 24g of titanium dioxide and 200mL of deionized water into a 500mL three-necked flask, mix well, then add concentrated hydrochloric acid dropwise to adjust the pH value to 5, raise the temperature to 65°C while stirring, slowly add a mixture of 10mL of DMSO and 1.2g of intermediate 2 into the above three-necked flask while stirring, keep warm and stir for 10h after adding, then cool to room temperature, filter the mixture, wash with anhydrous ethanol 5 times, and after washing, dry the product in vacuum at 80°C for 12h to obtain modified titanium dioxide.

[0034] Example 2

[0035] The specific steps of preparing antibacterial materials for shoes are as follows:

[0036] 70 parts of EPDM rubber, 10 parts of polyethylene, 20 parts of modified titanium dioxide obtained in Example 1, 10 parts of carbon black E250G and 0.5 parts of di-tert-butyl peroxide were mixed evenly and poured into an internal mixer, and internally kneaded at 100°C for 10 minutes; 0.5 parts of stearic acid, 1 part of zinc stearate and 0.5 parts of antioxidant D were added, the temperature was raised to 120°C, and the mixing was continued for 10 minutes to obtain a mixed rubber; finally, the temperature was raised to 150°C, 1 part of sulfur was added and vulcanized for 5 minutes, and after the vulcanization was completed, the mixture was melt-granulated and compression molded to obtain an antibacterial material for shoes.

[0037] Example 3

[0038] The specific steps of preparing antibacterial materials for shoes are as follows:

[0039] 78 parts of EPDM rubber, 15 parts of polyethylene, 26 parts of modified titanium dioxide obtained in Example 1, 16 parts of nano calcium carbonate and 0.6 parts of di-tert-butyl peroxide were mixed evenly and poured into an internal mixer, and internally kneaded at 105°C for 10 minutes; 1 part of stearic acid, 2 parts of zinc stearate and 1 part of antioxidant AW were added, the temperature was raised to 125°C, and the mixing was continued for 12 minutes to obtain a mixed rubber; finally, the temperature was raised to 155°C, 2 parts of sulfur were added and vulcanized for 6 minutes, and after the vulcanization was completed, melt granulation was performed, and compression molding was performed to obtain an antibacterial material for shoes.

[0040] Example 4

[0041] The specific steps of preparing antibacterial materials for shoes are as follows:

[0042] 80 parts of EPDM rubber, 20 parts of polyethylene, 30 parts of modified titanium dioxide obtained in Example 1, 5 parts of carbon black N234, 8 parts of nano calcium carbonate, 7 parts of fumed silica and 0.8 parts of di-tert-butyl peroxide were mixed evenly and poured into an internal mixer, and internally kneaded at 100-110°C for 10 minutes; 1.5 parts of stearic acid, 3 parts of zinc stearate and 1.5 parts of antioxidant RD were added, the temperature was raised to 130°C, and the mixing was continued for 15 minutes to obtain a mixed rubber; finally, the temperature was raised to 160°C, 3 parts of sulfur were added and vulcanized for 8 minutes, and after the vulcanization was completed, the mixture was melt-granulated and compression molded to obtain an antibacterial material for shoes.

[0043] Comparative Example 1

[0044] The specific steps of preparing shoe materials are as follows:

[0045] The remaining steps remain unchanged, and the modified titanium dioxide in Example 4 is removed to prepare the shoe material.

[0046] Comparative Example 2

[0047] The specific steps of preparing shoe materials are as follows:

[0048] The remaining steps remain unchanged, and the modified titanium dioxide in Example 4 is replaced by titanium dioxide without any treatment to prepare a shoe material.

[0049] Comparative Example 3

[0050] The specific steps of preparing shoe materials are as follows:

[0051] The remaining steps remain unchanged, the modified titanium dioxide in Example 4 is replaced by titanium dioxide without any treatment, and 1.5 parts of antibacterial agent didodecyl dimethyl ammonium chloride are added to prepare a shoe material.

[0052] Performance Testing

[0053] The tensile strength and elongation at break of the shoe materials prepared in Examples 2-4 and Comparative Examples 1-3 were tested, and a dry and wet accelerated aging test was performed using a xenon lamp aging test chamber. The aging test parameters were set as follows: the irradiation intensity was 75 W / m 2, the black mark temperature is 60±2℃, the dry-wet cycle is 100min illumination + 20min illumination and spraying, the total test time is 720h, and the tensile strength and elongation at break are tested after aging; the shoe materials prepared in Examples 2-4 and Comparative Examples 1-3 are made into test samples, placed in a special plastic bag, and then 1mL of inoculated bacterial solution is added, and air equivalent to the amount of inoculated bacterial solution is introduced into the plastic bag, the plastic bag is heat-sealed, and shaken at 37℃ for 24h, and the number of surviving bacteria is determined by the dilution plate culture method, and the antibacterial rate is calculated to test the antibacterial rate of the shoe materials against Escherichia coli and Staphylococcus aureus. And under the same conditions, the antibacterial rate of the shoe materials prepared in Examples 2-4 and Comparative Examples 1-3 is tested after 60 washes, and the test results are shown in the following table:

[0054]

[0055] “-” means no antibacterial effect.

[0056] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0057] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An antibacterial material for shoes, characterized in that: The invention comprises the following raw materials in parts by weight: 70-80 parts of EPDM rubber, 10-20 parts of polyethylene, 20-30 parts of modified titanium dioxide, 10-20 parts of reinforcing agent, 1.5-4.5 parts of lubricant, 1-3 parts of vulcanizing agent, 0.5-1.5 parts of antioxidant, and 0.5-0.8 parts of initiator; Wherein, the modified titanium dioxide is prepared by the following steps: S1, after nitrogen blowing into the flask, add 5-chloro-2-methyl-4-isothiazoline-3-one, triethylamine and DMSO, stir, add 3-butene-1-amine, react at 5°C for 8h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1; S2, under nitrogen protection, add intermediate 1, DBU and DMSO into a flask, stir, add coupling agent KH570, react at 60°C for 48h, and after the reaction, distill under reduced pressure to obtain intermediate 2; S3. Add titanium dioxide and deionized water into a flask, mix, then add concentrated hydrochloric acid to adjust the pH value to 5, raise the temperature to 65°C, add DMSO and intermediate 2, stir for 10 hours, cool, filter, wash, and dry to obtain modified titanium dioxide.

2. The antibacterial material for shoes according to claim 1, characterized in that: The amount of 5-chloro-2-methyl-4-isothiazoline-3-one, 3-butene-1-amine, triethylamine and DMSO in step S1 is 0.08 mol: 0.088 mol: 16 mL: 100 mL; the amount ratio of intermediate 1, coupling agent KH570, DBU and DMSO in step S2 is 0.07 mol: 0.075 mol: 2.1 mL: 130 mL; the mass ratio of titanium dioxide to intermediate 2 in step S3 is 20:

1.

3. The antibacterial material for shoes according to claim 1, characterized in that: The reinforcing agent is one or more of carbon black, nano calcium carbonate and fumed silica.

4. The antibacterial material for shoes according to claim 1, characterized in that: The lubricant is a mixture of stearic acid and zinc stearate in a mass ratio of 1:

2.

5. The antibacterial material for shoes according to claim 1, characterized in that: The vulcanizing agent is sulfur.

6. The antibacterial material for shoes according to claim 1, characterized in that: The antioxidant is one or more of antioxidant D, antioxidant SP, antioxidant AW, and antioxidant RD.

7. The antibacterial material for shoes according to claim 1, characterized in that: The initiator is di-tert-butyl peroxide.

8. The method for preparing an antibacterial material for shoes according to claim 1, characterized in that: The following steps are involved: Mix EPDM rubber, polyethylene, modified titanium dioxide, reinforcing agent and initiator evenly, pour into internal mixer, and mix at 100-110℃ for 10min; add lubricant and antioxidant, heat up to 120-130℃, continue mixing for 10-15min to obtain mixed rubber; finally heat up to 150-160℃, add vulcanizing agent and vulcanize for 5-8min, melt granulate after vulcanization, and compression mold to obtain antibacterial material for shoes.