Nonlinear conductive epoxy resin composite material constructed based on metal nanoparticles and silicon carbide particle filler, and preparation method and application thereof

The nonlinear conductive epoxy resin composite material constructed by metal nanoparticles and silicon carbide particle fillers solves the problems of low charge dissipation efficiency and barrier regulation under the influence of polymer thin layers, and achieves high-performance and flexible nonlinear conductive materials , suitable for electronic device packaging.

CN119060501AActive Publication Date: 2024-12-03SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411317348.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

The existing nonlinear conductive materials have low charge dissipation efficiency due to the influence of polymer thin layers under high electric fields, and are difficult to regulate the barrier height, which cannot meet the needs of high performance and flexible application.

Method used

Nonlinear conductive epoxy resin composite material constructed with metal nanoparticles and silicon carbide particle filler, silver nanoparticle-silicon carbide composite filler is formed through ultrasonic dispersion and high-temperature treatment, and combined with epoxy resin matrix to achieve efficient charge dissipation and adjustable potential Base height.

Benefits of technology

It achieves high nonlinear coefficient and rapid charge dissipation performance, effectively suppresses electrostatic discharge and local discharge, and is suitable for industrial applications of electronic device packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060501A_ABST
    Figure CN119060501A_ABST
Patent Text Reader

Abstract

The invention discloses a nonlinear conductive epoxy resin composite material constructed on the basis of metal nanoparticles and silicon carbide particle filler as well as a preparation method and application of the nonlinear conductive epoxy resin composite material. The nonlinear conductive epoxy resin composite material constructed by the metal nanoparticles and the silicon carbide particle filler comprises a functional filler composed of the metal nanoparticles and the silicon carbide material and an epoxy resin matrix, and the metal nanoparticles well dispersed on the surface of the silicon carbide material are used for guiding charge transport in the composite material. And a charge dissipation network is formed. The novel nonlinear conductive epoxy resin composite material disclosed by the invention has the capability of timely dissipating accumulated charges in a locally enhanced direct-current electric field, so that equipment is protected from being damaged by electrostatic discharge and partial discharge, and a new view angle and a new development direction are provided for an electronic device packaging material and an electrical equipment insulating material; and the material is simple in preparation process, high in operability and suitable for industrial popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonlinear conductive epoxy resin composite materials, and in particular to a preparation method and application of a nonlinear conductive epoxy resin composite material constructed based on metal nanoparticles and silicon carbide particle fillers. Background Art

[0002] The development of electronic components towards high integration and high power density poses severe challenges to the insulation performance and intelligence of their packaging materials. The design purpose of traditional packaging insulation materials is usually to improve the breakdown resistance. However, due to the complex structure of the device, electric field distortion and charge injection are inevitable. The accumulated free charge will cause electrostatic discharge or electron avalanche under long-term working conditions, resulting in insulation failure and threatening the safety of the components. In this case, a smart material whose electrical parameters are nonlinearly affected by the electric field intensity, namely nonlinear conductive materials, has attracted the attention of the industry. It has high insulation at low voltage, but can quickly release charge at high voltage to prevent local electric field distortion from causing insulation failure. The basic principle of the action of nonlinear materials is to achieve the insulation-conductivity state conversion through the Schottky barrier of wide bandgap semiconductor materials. Limited by the scarcity of wide bandgap semiconductors (such as zinc oxide and silicon carbide), many people have proposed to adjust the barrier height by constructing core-shell structures (such as bismuth oxide / zinc oxide, titanium dioxide / barium titanate, silicon dioxide / silicon carbide), hoping to obtain adjustable threshold field strength and nonlinear conductivity. However, this strategy places strict requirements on the conductivity of the shell components. On the one hand, a highly insulating shell will lead to a decrease in the charge dissipation efficiency above the threshold field strength. On the other hand, a shell with low resistivity is difficult to maintain ideal insulating protection below the threshold electric field because the charges tend to be conducted along the shell rather than through the semiconductor core. In addition, even if the filler filling amount has reached the percolation threshold, there is still a polymer matrix layer with a thickness of about 15 nanometers between adjacent fillers. This situation is usually ignored in the design of nonlinear materials in the past. The resulting additional polymer / semiconductor interface seriously affects the charge dissipation efficiency under high electric fields. Therefore, it is still difficult to prepare nonlinear conductive materials with high performance and adjustable parameters.

[0003] In the past, the preparation schemes for high-performance nonlinear conductive materials are disclosed in patents CN114854177B and CN115536982B. CN114854177B uses a silane coupling agent to modify silicon carbide to improve its compatibility with the epoxy resin matrix. However, its nonlinear coefficient is only increased to 5.6, and the negative impact of the polymer thin layer between the filler particles cannot be solved. CN115536982B uses dopamine and titanium dioxide to jointly modify barium carbonate particles. However, due to the shielding effect of the dopamine layer on the carriers in the titanium dioxide region, the performance of the prepared nonlinear conductive material is difficult to control and cannot meet the flexible needs of practical applications.

[0004] In summary, it is very important to solve the problem of barrier height regulation, inhibit the adverse effects of polymer thin layers on charge dissipation rate, and develop a high-performance nonlinear conductive composite material with adjustable barrier height and high nonlinear coefficient, which provides a promising direction for the development of intelligent packaging materials for the new generation of electronic devices. Summary of the invention

[0005] The purpose of the present invention is to provide a nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers, and a preparation method and application thereof.

[0006] The technical solution adopted by the present invention is: A nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers comprises an epoxy resin matrix and a metal nanoparticle-silicon carbide composite filler. The metal nanoparticle-silicon carbide composite filler comprises micron-sized silicon carbide microspheres and metal nanoparticles dispersed and attached on the outer surface thereof.

[0007] Furthermore, the volume fraction of silicon carbide is 20-25 vol%, and the volume fraction of metal nanoparticles is 0.2-0.6 vol%; the particle size of silicon carbide particles in the nonlinear conductive epoxy resin composite material constructed based on metal nanoparticles and silicon carbide particle fillers is in the range of 4-7 microns, and the particle size of the metal nanoparticles is in the range of 8-60 nanometers.

[0008] Silver nanoparticle-silicon carbide composite filler is prepared by the following method: 1) First, silicon carbide particles are mixed in deionized water, and a silicon carbide dispersion is obtained by ultrasonic dispersion, wherein the mass fraction of silicon carbide is 0.047-0.141, silver nitrate or gold chlorate powder is added and stirred to obtain a silicon carbide-metal salt mixed solution, and the solution is allowed to react for 15-60 minutes; the mass ratio of silver nitrate to silicon carbide in the mixed solution is 0.034-0.102, and the mass ratio of gold chlorate to silicon carbide is 0.068-0.204; 2) filtering the reaction solution, freeze-drying the solid matter to obtain a composite filler having metal nanoparticles and silicon carbide particles in contact with each other; 3) The composite filler in which the metal nanoparticles and the silicon carbide particles are in contact with each other after freeze-drying is subjected to high temperature treatment for 2-4 hours to obtain a silver nanoparticle-silicon carbide composite filler in which the metal nanoparticles and the silicon carbide particles are in close contact with each other.

[0009] Furthermore, in step 1), the ultrasonic dispersion time is 20-60 minutes.

[0010] Furthermore, in step 2), the silicon carbide-silver nitrate mixed solution needs to be kept away from light for reaction for 15-60 minutes, and then quickly filtered.

[0011] Furthermore, in step 3), the high temperature treatment process needs to be carried out under a nitrogen atmosphere, and the heating temperature is 300-360°C, preferably 360°C.

[0012] The particle size of the obtained metal nanoparticles is regulated by the static reaction time of the silicon carbide-metal salt mixed solution, and the particle size of the metal nanoparticles is in the range of 8-60 nanometers.

[0013] The preparation method of the nonlinear conductive epoxy resin composite material constructed based on metal nanoparticles and silicon carbide particle fillers comprises the following steps: dispersing the silver nanoparticle-silicon carbide composite fillers obtained at different reaction times in a mixture of epoxy resin, curing agent and accelerator for degassing and high-temperature curing to obtain the corresponding composite material.

[0014] The epoxy resin monomer, curing agent, accelerator and metal nanoparticle-silicon carbide composite filler are added in the following proportions: 1 part of epoxy resin monomer, 1-1.2 parts of curing agent, 0.006-0.01 parts of accelerator, 8.2-10.28 parts of metal nanoparticle-silicon carbide composite filler, and the volume fraction of metal nanoparticle-silicon carbide composite filler in the prepared composite material is 20%-25%. The epoxy resin is at least one of alicyclic epoxy resin and bisphenol A epoxy resin; the curing agent is methyl hexahydrophthalic anhydride; and the accelerator is 2-ethyl-4-methylimidazole.

[0015] Furthermore, the dispersion conditions are as follows: firstly, the nanoparticle-silicon carbide composite filler is ultrasonically dispersed in acetone for 30 minutes, and after the epoxy resin is added, the mixture is heated and stirred in an oil bath for 4 hours to evaporate the acetone.

[0016] Furthermore, the high temperature curing conditions are: first curing at 95°C-115°C for 40-80 minutes, then curing at 115°C-125°C for 100-150 minutes, and then curing at 135°C-145°C for 30-60 minutes.

[0017] The nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers prepared by the present invention has a volume fraction of SiC of 20-25 vol%; a volume fraction of metal nanoparticles of 0.2-0.6 vol%, and a particle size of silicon carbide particles in the nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers in the range of 4-7 microns. The particle size of the metal nanoparticles is in the range of 8-60 nanometers.

[0018] The nonlinear conductive epoxy resin composite material constructed based on metal nanoparticles and silicon carbide particle fillers of the present invention includes an epoxy resin matrix, a functional filler composed of metal nanoparticles and silicon carbide materials, and uses a highly engineering solution reduction method to process silicon carbide to realize metal nanoparticles of different particle sizes on its surface, and uses metal nanoparticles well dispersed on the surface of silicon carbide material to guide charge transport inside the composite material, forming a charge dissipation network, and giving the composite material the performance of efficient charge dissipation under high electric fields. The nonlinear conductive epoxy resin composite material constructed based on metal nanoparticles and silicon carbide particle fillers of the present invention has a high nonlinear coefficient, that is, the insulating-conductive state conversion under high and low electric field conditions is obvious, and it has a rapid charge dissipation ability under locally enhanced electric field conditions, preventing electrostatic discharge and local discharge hazards caused by charge accumulation. The new nonlinear conductive material provides a promising direction for electronic intelligent packaging, and the process has stronger operability and is suitable for industrial application. The material of the present invention can be used to prepare electronic device packaging materials.

[0019] Compared with the prior art, the advantages and beneficial effects of the present invention are: (1) The present invention directly utilizes the Schottky barrier formed at the metal-semiconductor interface by constructing a contact between metal nanoparticles and silicon carbide, thereby achieving flexible regulation of the barrier height by screening metal materials.

[0020] (2) The metal nanoparticles prepared by the solution reduction method of the present invention grow in situ on the surface of silicon carbide particles, avoiding large-scale agglomeration and not deteriorating the insulation properties of the composite material finally prepared under low electric fields.

[0021] (3) The metal nanoparticles used in the present invention utilize the electric field near the distortion of the metal material to overcome the influence of the polymer thin layer, so that the final prepared composite material has the ability to quickly dissipate charge under high electric field conditions, thereby protecting the equipment from the hazards of electrostatic discharge and local discharge.

[0022] (4) The nonlinear coefficient of the present invention reaches 8.7 when the filler volume fraction is 25 vol%, and it exhibits rapid charge dissipation performance in the electrostatic discharge test, effectively suppressing the accumulated charge on the material surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a schematic diagram of the preparation process of the nonlinear conductive epoxy resin composite material based on silver metal nanoparticles and silicon carbide particle fillers.

[0024] Figure 2 This is the SEM image of silver metal nanoparticles-silicon carbide composite filler.

[0025] Figure 3This is the ultraviolet photoelectron spectrum of silver metal nanoparticles-silicon carbide composite filler.

[0026] Figure 4 This is the post-processed image of the UV-visible diffuse reflectance spectrum of silver metal nanoparticles-silicon carbide composite filler.

[0027] Figure 5 The relative energy band structure diagram of silicon carbide, silver, gold and composite fillers of two metal nanoparticles and silicon carbide.

[0028] Figure 6 This is a graph showing the test results of electrical conductivity-electric field strength of a composite material prepared by directly filling silicon carbide with a composite filler of two metal nanoparticles and silicon carbide.

[0029] Figure 7 Simulation results of the internal electric field intensity distribution and electrical conduction path of a nonlinear conductive epoxy resin composite material based on silver metal nanoparticles and silicon carbide particle fillers Figure 8 These are SEM images of silver metal nanoparticle-silicon carbide composite fillers with reaction growth times of 15, 40, and 60 minutes, respectively.

[0030] Fig. 9 To verify the electrostatic discharge test results of the composite materials filled with metal nanoparticles-silicon carbide composite fillers and directly filled with silicon carbide to dissipate charge.

[0031] Fig.10 The conductivity-electric field strength test graph of the nonlinear conductive composite materials EP-Ag40 / SiC and EP-SiC prepared in Example 2 and Comparative Example 1. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further explained below in conjunction with specific embodiments and drawings.

[0033] Example 1 A nonlinear conductive epoxy resin composite material based on silver metal nanoparticles and silicon carbide particle fillers, the preparation method of which comprises the following steps (preparation process as shown in Figure 1 shown): 1) Add silicon carbide powder to deionized water for ultrasonic dispersion for 45 minutes, the mass ratio of silicon carbide to deionized water is 5:100, add silver nitrate powder to the above silicon carbide dispersion, the mass ratio of silver nitrate powder to deionized water is 0.17:100, stir and dissolve thoroughly, then add 1 mol / L sodium hydroxide solution dropwise to make the pH value reach 12, and place in a dark place for reaction for 60 minutes; 2) The solution after the reaction was filtered, washed with water and ethanol three times respectively, and freeze-dried at a freezing temperature of -25°C for 24 hours. After the freeze-drying was completed, the powder sample was removed and heated at 360°C in a tube furnace in a nitrogen atmosphere for 4 hours; 3) Repeat the above steps to obtain a sufficient amount of silver metal nanoparticle-silicon carbide composite filler, add 20.59 grams of composite filler into 20 grams of acetone, disperse it by ultrasonication for 45 minutes, then add 10 grams of alicyclic epoxy resin, heat to 70°C and stir for 4 hours to evaporate all the acetone. Add methyl hexahydrophthalic anhydride and 2-ethyl-4-methylimidazole in a mass ratio of 1:1.2:0.006, stir for 30 minutes, place in a vacuum box at 50°C and evacuate for 5 hours to remove bubbles in the mixture, then place in a heating box, cure at 110°C for 60 minutes, then cure at 125°C for 120 minutes, and then cure at 135°C for 60 minutes to obtain a nonlinear conductive epoxy resin composite material based on silver metal nanoparticles and silicon carbide particle fillers (denoted as EP-Ag60 / SiC), and the volume fraction of fillers inside the composite material is 25vol%.

[0034] Example 2 A nonlinear conductive epoxy resin composite material based on silver metal nanoparticles and silicon carbide particle fillers, denoted as EP-Ag40 / SiC, is prepared in the same manner as in Example 1 except that the light-proof reaction time of the solution is adjusted to 40 minutes in step 1).

[0035] Example 3 A nonlinear conductive epoxy resin composite material based on silver metal nanoparticles and silicon carbide particle fillers, denoted as EP-Ag15 / SiC, is prepared in the same manner as in Example 1 except that the light-proof reaction time of the solution is adjusted to 15 minutes in step 1).

[0036] Example 4 A nonlinear conductive epoxy resin composite material based on gold nanoparticles and silicon carbide particle fillers, denoted as EP-Au60 / SiC, is prepared in the same manner as in Example 1, except that the added metal particle salt is changed from silver nitrate to gold chlorate in step 1), and the mass ratio of the added gold chlorate powder to deionized water is 0.34:100.

[0037] Comparative Example 1 A directly silicon carbide filled epoxy composite material, the preparation method of which comprises the following steps: 20.59 grams of composite filler was added to 20 grams of acetone, and ultrasonic dispersion was performed for 45 minutes. Then, 10 grams of alicyclic epoxy resin was added, and the mixture was heated to 70°C and stirred for 4 hours to evaporate all the acetone. Methyl hexahydrophthalic anhydride and 2-ethyl-4-methylimidazole were added in a mass ratio of 1:1.2:0.006 for alicyclic epoxy resin, methyl hexahydrophthalic anhydride and 2-ethyl-4-methylimidazole. After stirring for 30 minutes, the mixture was placed in a vacuum box at 50°C and vacuumed for 5 hours to remove bubbles in the mixture. The mixture was then placed in a heating box and cured at 110°C for 60 minutes, then at 125°C for 120 minutes, and then at 135°C for 60 minutes to obtain a directly filled silicon carbide epoxy resin composite material (denoted as EP-SiC), and the volume fraction of filler inside the composite material was 25 vol%.

[0038] Performance Testing 1. The TEM image of the silver nanoparticle-silicon carbide composite filler prepared in Example 1 is as follows: Figure 2 As shown, the infrared spectrum is Figure 3 As shown, the thermal gravimetric curve is Figure 4 shown.

[0039] Depend on Figure 2 It can be seen that the high-angle annular dark field scanning image clearly depicts the presence of silver metal nanoparticles attached to the surface of silicon carbide. Among them, the smaller particles are uniformly spherical, while the particles with larger diameters have different shapes. The reason for this phenomenon is that the nanoparticles that are close to each other during the growth stage will contact and grow into irregular elliptical spheres. However, overall, there is no obvious agglomeration phenomenon.

[0040] 2. The ultraviolet photoelectron spectra of silicon carbide and the composite fillers of silver and gold nanoparticles and silicon carbide prepared in Examples 1 and 4 (referred to as SiC, Ag / SiC and Au / SiC) are as follows: Figure 3 shown.

[0041] The UV photoelectron spectra obtained in SiC, Ag / SiC, and Au / SiC highlight low and high binding energy regions. The low and high binding energy cutoffs are determined based on the corresponding tangents in each region and are used to determine the Fermi level, valence band maximum, and conduction band minimum (relative to the vacuum level) for each material. The calculated Fermi level of silicon carbide is 3.01 eV, and the Fermi levels of silicon carbide composite fillers with metal nanoparticles on the surface are all higher. This is due to the large work functions of silver and gold, 4.26 and 5.1, respectively, which makes it more difficult for electrons to be excited to the vacuum level.

[0042] 3. The post-processing diagram of the UV-visible diffuse reflectance spectra of the composite fillers of silicon carbide and the silver and gold nanoparticles and silicon carbide prepared in Examples 1 and 4 is as follows: Figure 4 shown.

[0043] The band gaps of SiC, Ag / SiC and Au / SiC were determined by UV-visible testing and subsequent processing. The Tauc fitting result graph shows that the band gaps of SiC, Ag / SiC and Au / SiC are 2.85 eV, 2.58 eV and 2.72 eV, respectively. Compared with Au / SiC, Ag / SiC has a smaller band gap because of the higher conductivity of silver metal. Ag / SiC and Au / SiC show a new peak in the low photon energy range, at 1.04 eV and 1.13 eV, respectively. This peak is caused by the stimulation of electrons from low-energy metal nanoparticle clusters.

[0044] 4. The relative band structures of the composite fillers of silicon carbide and the silver and gold nanoparticles and silicon carbide prepared in Examples 1 and 4 are as follows: Figure 5 shown.

[0045] As shown in the figure, the conduction band bottom and valence band top of Ag / SiC and Au / SiC are higher than those of SiC. In addition, the Fermi level of Ag / SiC and Au / SiC is between the Fermi level of silicon carbide and metal materials. This is because when metal and silicon carbide contact to form a heterojunction, the band structure will undergo new changes due to the Fermi level alignment effect. Since silicon carbide has a weak binding force with electrons, electrons migrate, forming a space charge region on the interface. Therefore, this leads to band bending. Electrons passing through the metal-silicon carbide interface must overcome the Schottky barrier on the interface.

[0046] 5. The conductivity-electric field strength test results of the epoxy resin composite materials (i.e., EP-Ag60 / SiC, EP-Au60 / SiC and EP-SiC) prepared in Examples 1, 4 and Comparative Example 1 are as follows: Figure 6 shown.

[0047] The nonlinear conductive behavior of nonlinear conductive composite materials is usually evaluated by switching electric field and nonlinear coefficient, which represent the potential application range and nonlinear effect. The fitting results show that the nonlinear coefficients of EP-Ag60 / SiC and EP-Au60 / SiC are 8.7 and 8.2, respectively, which are significantly higher than EP-SiC (7.8). At the same time, the switching electric fields of EP-Ag60 / SiC and EP-Au60 / SiC are 1.11 kV / mm and 1.07 kV / mm, respectively, which are significantly lower than EP-SiC (3kV / mm). This improves the sensitivity of nonlinear conductive materials to electric fields and can dissipate accumulated charges more sensitively. The conductivity of the composite material with metal nanoparticles is significantly improved, indicating that it is more sensitive to electric fields. This feature can quickly remove the charges accumulated on the surface of the material, thereby avoiding more serious partial discharge. This phenomenon can be explained by the presence of metal nanoparticles on the surface of silicon carbide, which is a sensitive micro-capacitor structure that can significantly change the electric field strength of the nearby polymer. When electrons reach the closest metal nanoparticles on the adjacent silicon carbide particles, they can easily cross the polymer for hopping conduction. Compared with composite materials directly filled with silicon carbide, metal nanoparticles make it easier to form a complete conduction channel. The barrier height at the interface between metal nanoparticles and silicon carbide plays an important role in nonlinear electrical properties. Interfaces with higher barrier heights require greater energy to pass through. Therefore, choosing a metal with higher conductivity and smaller work function to build on the semiconductor surface will result in a significant reduction in the switching electric field value.

[0048] 6. The phase field simulation results of the internal electrical process of the EP-Ag60 / SiC composite material prepared in Example 1 under the action of DC voltage are shown in Figure 7 shown.

[0049] To further investigate the effect of metal nanoparticles on the nonlinear conductive properties of the composite material, we established a phase model to simulate the diffusion of the electrical channel. Due to the different electrical conductivity and relative dielectric constant between silver metal and polymer materials, a strong and concentrated electric field enhancement effect will appear near the silver metal nanoparticles. It is worth noting that the electric field distortion in the polymer region between adjacent metal nanoparticles is more significant. Therefore, electrons will tend to pass through silicon carbide through silver metal nanoparticles, thereby promoting the directional movement of electrons and the appearance of the most potential barriers along the conduction channel at the metal-silicon carbide interface. This conclusion can be verified by the conductivity path simulation results.

[0050] 7. The SEM results of the silver metal nanoparticle-silicon carbide composite fillers (i.e., Ag60 / SiC, Ag40 / SiC and Ag15 / SiC) prepared in Examples 1, 2 and 3 are as follows: Figure 8 shown.

[0051] By changing the reaction time, silver metal nanoparticles of different sizes can be synthesized on the silicon carbide surface. Figure 8 The close relationship between growth time and metal nanoparticle diameter is shown. Nanoparticles with smaller diameters present a more uniform spherical shape. The reason for this phenomenon is that during the static reaction stage, the silver atoms produced by ion reduction first combine with silicon carbide. As the number of silver atoms gradually increases, the size of the nanoparticles also increases. When two adjacent clusters of silver atoms come into contact, agglomeration occurs. Therefore, silver metal nanoparticles that react for 60 minutes lose their unique spherical morphology, while at reaction durations of 40 minutes and 15 minutes, the aggregation phenomenon is reduced, causing the nanoparticles to maintain their spherical morphology.

[0052] 8. The test results of the conductivity-electric field strength of the nonlinear conductive composite materials (i.e., EP-Ag60 / SiC, EP-Ag40 / SiC and EP-Ag15 / SiC) prepared in Examples 1, 2 and 3 are as follows: Fig. 9 shown.

[0053] Compared with EP-Ag60 / SiC, EP-Ag40 / SiC shows more prominent nonlinear conductivity, while EP-Ag15 / SiC shows the opposite trend. This phenomenon can be attributed to the fact that a large number of nanoparticles in Ag15 / SiC are smaller than the threshold size for the Coulomb blockade effect to occur, thus limiting the electron transport process. The nanoparticle size distribution of Ag15 / SiC was determined by a normal distribution with a mean value of 13.2 nm, which is consistent with previous studies on the nanoparticle size affected by the Coulomb blockade effect.

[0054] 9. The conductivity-electric field strength test results of the nonlinear conductive composite materials (i.e., EP-Ag40 / SiC and EP-SiC) prepared in Example 2 and Comparative Example 1 are as follows: Fig.10 shown.

[0055] In order to evaluate the electrostatic discharge protection capability of the nonlinear conductive composite material proposed in this patent, we verified its adaptive charge release behavior under the charge pulse generated by the electrostatic discharge gun. When the discharge pulse acts on the surface of the material, if the sample is in a state of increased conductivity, the charge will flow into the ground electrode through body conduction. Otherwise, the charge will gradually dissipate through the bypass resistor. Therefore, the adaptive charge release characteristics of the material are mainly affected by its nonlinear conductivity, especially the switching electric field. When subjected to a charge pulse of 40 nC, the electric field on the EP-Ag40 / SiC sample is 1 kV / mm, which is lower than the switching electric field of 1.2kV / mm. Therefore, the material is in an insulating state and the charge dissipates slowly. In contrast, when the applied charge pulse increases to 80 nC (corresponding to an electric field strength of 2 kV / mm on the sample, exceeding the switching electric field), the conductive path within the EP-Ag40 / SiC is activated and the conductivity rises sharply. Therefore, the charge on the surface is rapidly reduced, suppressing the generation of overvoltage. Compared with EP-SiC, its charge dissipation rate is significantly improved. Additionally, the charge dissipation behavior is consistent with the relative magnitude of the conductivity. In the same amount of time, EP-SiC accumulates more surface charge than EP-Ag40 / SiC. These results suggest that EP-Ag40 / SiC, which has significant nonlinear conductivity, tends to dissipate charge faster when exposed to electrostatic hazards, thereby reducing the likelihood of electronic component failure.

Claims

1. A nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers, characterized in that: The composite material is composed of an epoxy resin matrix and a metal nanoparticle-silicon carbide composite filler; the metal nanoparticle-silicon carbide composite filler comprises silicon carbide particles and metal nanoparticles prepared by a solution reduction method.

2. The nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers according to claim 1, characterized in that: The volume fraction of silicon carbide is 20-25 vol%, and the volume fraction of metal nanoparticles is 0.2-0.6 vol%; the particle size of silicon carbide particles in the nonlinear conductive epoxy resin composite material constructed based on metal nanoparticles and silicon carbide particle fillers is in the range of 4-7 microns, and the particle size of the metal nanoparticles is in the range of 8-60 nanometers.

3. The method for preparing the nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers according to any one of claims 1 to 2, characterized in that: The following steps are involved: The metal nanoparticle-silicon carbide composite filler is mixed into a mixture of epoxy resin monomer, curing agent and accelerator, and after degassing and curing, a nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers is obtained; The proportion of epoxy resin monomer, curing agent, accelerator and metal nanoparticle-silicon carbide composite filler added is as follows: 1 part of epoxy resin monomer, 1-1.2 parts of curing agent, 0.006-0.01 parts of accelerator, 8.2-10.28 parts of metal nanoparticle-silicon carbide composite filler, and the volume fraction of metal nanoparticle-silicon carbide composite filler in the prepared composite material is 20%-25%.

4. The preparation method according to claim 3, characterized in that: The epoxy resin is at least one of alicyclic epoxy resin and bisphenol A epoxy resin; the curing agent is methyl hexahydrophthalic anhydride; and the accelerator is 2-ethyl-4-methylimidazole.

5. The preparation method according to claim 3, characterized in that: The curing conditions are: first curing at 95°C-115°C for 40-80 minutes, then curing at 115°C-125°C for 100-150 minutes, and then curing at 135°C-145°C for 30-60 minutes.

6. The nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers according to claim 3, characterized in that: Silver nanoparticle-silicon carbide composite filler is prepared by the following method: 1) firstly, silicon carbide particles are mixed in deionized water, and a silicon carbide dispersion is obtained by ultrasonic dispersion, wherein the mass fraction of silicon carbide is 0.047-0.141, silver nitrate or gold chlorate powder is added and stirred to obtain a silicon carbide-metal salt mixed solution, and the solution is allowed to stand for reaction for 15-60 minutes; the mass ratio of silver nitrate to silicon carbide in the mixed solution is 0.034-0.102, and the mass ratio of gold chlorate to silicon carbide is 0.068-0.204; 2) filtering the reaction solution, and freeze-drying the solid to obtain a composite filler having metal nanoparticles and silicon carbide particles in contact with each other; 3) The composite filler in which the metal nanoparticles and the silicon carbide particles are in contact with each other after freeze-drying is subjected to high temperature treatment for 2-4 hours to obtain a silver nanoparticle-silicon carbide composite filler in which the metal nanoparticles and the silicon carbide particles are in close contact with each other.

7. The nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers according to claim 6, characterized in that: In step 2), the silicon carbide-silver nitrate mixed solution needs to be kept away from light for reaction for 15-60 minutes, and then quickly filtered.

8. The nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers according to claim 6, characterized in that: In step 3), the process is carried out under a nitrogen atmosphere, and the heating temperature is 300-360°C.

9. The nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers according to claim 6, characterized in that: The particle size of the obtained metal nanoparticles is regulated by the static reaction time of the silicon carbide-metal salt mixed solution, and the particle size of the metal nanoparticles is in the range of 8-60 nanometers.

10. Use of the nonlinear conductive epoxy resin composite material based on metal nanoparticles and silicon carbide particle fillers as claimed in claim 1 or 2 in the preparation of electronic device packaging materials and high-voltage DC electrical equipment insulation.

Citation Information

Patent Citations

  • An epoxy composite material with nonlinear conductivity and dielectric properties, its preparation method and application

    CN115536982B

  • An instrument for filling an injection syringe

    EP0000465A1

  • Organophosphonic ester compounds, process for their preparation and their utilisation as insecticides, acaricides and nematocides

    EP0000528A1

  • Tree-like structure micro-nano wave absorption agent / epoxy resin composite wave absorption material preparation method

    CN103408899A

  • Epoxy resin composite insulating material with nonlinear conductivity and preparation method thereof

    CN107266863A

Cited By

  • Capacitive bushing for high-insulativity photovoltaic power grid and manufacturing method of capacitive bushing

    CN120954838A