Glass fiber reinforced resin-based composite material and preparation method thereof
Through winding molding and photocuring technology, multifunctional vinyl ester resin and glass fiber tows are used to form high-performance glass fiber reinforced resin-based composite materials, solving the problems of high energy consumption and insufficient performance in traditional processes and achieving high efficiency , environmentally friendly composite material preparation, suitable for a variety of high-performance applications.
Patent Information
- Application Number
- CN202411046691.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-12-03
AI Technical Summary
The molding process of traditional fiber-reinforced resin-based composites has problems such as high energy consumption, long production cycles and large environmental pollution. The application of some non-heat-resistant materials is limited, and a new generation of curing molding process is needed to improve production efficiency and material performance. .
The glass fiber reinforced resin matrix composite material is prepared by winding molding and photocuring technology to form a high-performance three-dimensional crosslinking network structure. Improve the mechanical properties and heat resistance of the material.
Significantly improves the production efficiency of glass fiber reinforced resin-based composite materials, reduces energy consumption, ensures high performance and dimensional stability of the products, the tensile strength reaches 773MPa, and the tensile modulus reaches 23.14GPa, suitable for high-performance pressure vessels and pipeline production.
Smart Images

Figure BDA0004973676610000091 
Figure BDA0004973676610000092 
Figure BDA0004973676610000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of composite material preparation, and in particular, relates to a glass fiber reinforced resin-based composite material and a preparation method thereof. Background Art
[0002] Fiber reinforced resin composites (FRP) are high-performance materials composed of fiber reinforcement and resin matrix. They are widely used in aerospace, transportation, military and other fields due to their light weight, high strength and corrosion resistance. The current conventional molding process for this type of material is thermal curing and thermoplastic methods. While these traditional methods are widely used, they have significant defects such as high energy consumption, long production cycle and greater environmental pollution. In addition, the application of some non-heat-resistant materials as matrices is also limited. Therefore, the development of a new generation of curing molding processes for fiber reinforced resin composites has great social and economic value. Summary of the invention
[0003] In view of the defects of the traditional hot forming process, the present invention provides a glass fiber reinforced resin-based composite material and a preparation method thereof, which can not only significantly improve the production efficiency of the glass fiber reinforced resin-based composite material and reduce the energy consumption in the curing and forming process, but also effectively ensure the high performance of the product by the high-precision and stable forming process. Specifically, the Tg of the resin matrix in the photocurable composite material obtained by the present invention can reach 87.7°C, indicating that the resin matrix has good heat resistance and dimensional stability; at the same time, the tensile strength of the glass fiber reinforced resin-based composite material obtained by the present invention can reach 773MPa, and the tensile modulus can reach 23.14GPa, indicating that the composite unidirectional plate has excellent mechanical properties.
[0004] A first aspect of the present invention provides a method for preparing a glass fiber reinforced resin-based composite material, comprising:
[0005] (1) mixing a multifunctional vinyl ester resin, a reactive diluent and an ultraviolet light initiator to prepare a matrix;
[0006] (2) using a winding device to impregnate the glass fiber bundle with the substrate and then wind it onto the mold;
[0007] (3) removing the wound sample obtained in step (2) from the mold and performing photocuring to obtain a composite material.
[0008] Furthermore, the mass ratio of the multifunctional vinyl ester resin, the reactive diluent, the ultraviolet light initiator and the glass fiber bundle is (20-40): (5-15): (0.5-2): (30-50).
[0009] Furthermore, in step (1), the multifunctional vinyl ester resin, the reactive diluent and the ultraviolet light initiator are mixed to prepare a matrix, which includes: the multifunctional vinyl ester resin, the reactive diluent and the ultraviolet light initiator are mixed, subjected to ultrasonic treatment and heating, and then degassed in a vacuum drying oven to obtain the matrix.
[0010] Furthermore, the heating temperature is 40-60°C.
[0011] Furthermore, the ultrasonic treatment time is 20 min-30 min.
[0012] Furthermore, the vacuum degree of the degassing process is -0.1 to -0.3 MPa, and the processing time is 20 min to 30 min.
[0013] Furthermore, in step (1), an auxiliary agent may be added during the mixing of the multifunctional vinyl ester resin, the reactive diluent and the ultraviolet light initiator, wherein the auxiliary agent includes at least one of a toughening agent, a defoaming agent and an antioxidant.
[0014] Furthermore, in step (1), the multifunctional vinyl ester resin includes at least one of bisphenol A epoxy acrylate, novolac epoxy acrylate, epoxidized oil acrylate and modified epoxy acrylate.
[0015] Furthermore, in step (1), the reactive diluent includes at least one of a monofunctional acrylate derivative, a difunctional acrylate derivative, and a multifunctional acrylate derivative.
[0016] Furthermore, in step (1), the ultraviolet light initiator comprises at least one of acylphosphine oxides, benzophenone compounds and benzil compounds.
[0017] Furthermore, in step (2), the glass fiber bundle includes at least one of E-glass fiber, C-glass fiber and high-strength glass fiber.
[0018] Further, in step (2), the parameters of the winding device include at least one of the following:
[0019] The winding method of the winding device is hoop winding;
[0020] The number of winding layers of the glass fiber bundle is 2 to 4;
[0021] The advancing distance of the glass fiber bundle is 40 to 200 mm;
[0022] The stepping of the glass fiber bundle is 0.5 to 0.8 times the width of a single bundle yarn sheet;
[0023] The winding tension of the glass fiber bundle is 0 to 100N;
[0024] The winding rate of the glass fiber bundle is 10-40° / min.
[0025] Furthermore, in step (3), the photocuring includes: removing the wound sample obtained in step (2) from the mold and transferring it to an ultraviolet lamp device for photocuring.
[0026] Furthermore, before curing the wound sample, a transparent adhesive paper or a transparent glass plate is fixed on the surface of the sample in advance.
[0027] Furthermore, the ultraviolet light wavelength range of the ultraviolet lamp device is 320-400nm; and / or the irradiation power of the ultraviolet lamp device is 100-200W; and / or the irradiation distance of the ultraviolet lamp device is 5-30cm; and / or the irradiation time of the ultraviolet lamp device is 1-2min; the ambient temperature of the photocuring process is 20-50°C.
[0028] A second aspect of the present invention provides a glass fiber reinforced resin-based composite material, which is prepared by the method described in the first aspect.
[0029] Compared with the prior art, the present invention has at least the following beneficial effects:
[0030] (1) The present invention uses multifunctional vinyl ester resin, reactive diluent, ultraviolet light initiator and glass fiber as raw materials to prepare glass fiber reinforced resin-based composite materials, which can improve the three-dimensional cross-linked network structure of the matrix, so that the mechanical properties, heat resistance, dimensional stability and other properties of the resin matrix are improved, thereby giving the composite material more excellent comprehensive performance.
[0031] (2) The present invention provides a method for preparing a glass fiber reinforced resin-based composite material by winding molding and ultraviolet light curing. This method can not only significantly improve the production efficiency of the glass fiber reinforced resin-based composite material and reduce the energy consumption in the curing molding process, but also ensure a stable molding process and easy control of the surface accuracy of the product.
[0032] (3) The present invention combines winding molding technology with light curing technology, expanding the rapid prototyping method of fiber-reinforced resin-based composite materials, and this method is expected to be applied to the production process of pressure vessels and pipelines in the fields of construction, transportation, military industry, etc. Specific implementation methods
[0034] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments, and the following examples are only descriptive, not restrictive, and cannot be used to limit the scope of protection of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] The technical solution of the present application is based on the following principles: the photocuring reaction is a chemical reaction initiated by a light source with a certain amount of energy, and the reaction system is composed of a monomer or oligomer, an active diluent and a photoinitiator. The ground state molecule of the initiator absorbs light energy and undergoes an electronic transition to become an excited state molecule. The excited state molecule cannot exist stably due to its high energy, and a part of it is inactivated, while the other part undergoes electron and energy transfer to become an active species. The free radical photoinitiator can produce free radical active species, inducing the vinyl ester resin to undergo an addition reaction on the carbon-carbon double bond (C=C), and then cross-linking to form a three-dimensional network molecular structure. Since the key to photocuring technology is the light source irradiation process, glass fiber with high light transmittance, excellent comprehensive performance and good processing performance is an excellent reinforcing fiber for photocuring composite materials. At the same time, the photocuring technology with high processing efficiency can be matched with a winding molding process suitable for continuous production and high degree of automation, providing a new method for the rapid prototyping technology of glass fiber reinforced resin-based composite materials.
[0036] A first aspect of the present invention provides a method for preparing a glass fiber reinforced resin-based composite material. According to an embodiment of the present invention, the method comprises:
[0037] S1: Mixing a multifunctional vinyl ester resin, a reactive diluent and a UV photoinitiator to prepare a matrix
[0038] Specifically, multifunctional vinyl ester resin (VE) has the characteristics of both unsaturated resin and epoxy resin, and the double bonds at both ends of the molecular chain are extremely active, so that the vinyl resin can be quickly cured to form a highly cross-linked rigid network structure, so that it has good mechanical properties and corrosion resistance. On the one hand, the active diluent can adjust the viscosity of the system to improve its photocuring performance, and on the other hand, it can adjust the network structure of the resin after curing to change its mechanical properties. The present invention uses multifunctional vinyl ester resin, active diluent, ultraviolet light initiator and glass fiber as raw materials to prepare glass fiber reinforced resin-based composite materials, which can improve the three-dimensional cross-linked network structure of the matrix, so that the mechanical properties, heat resistance, dimensional stability and other properties of the resin matrix are improved, thereby giving the composite material more excellent comprehensive performance.
[0039] According to one embodiment of the present invention, the matrix prepared by mixing the multifunctional vinyl ester resin, the reactive diluent and the ultraviolet light initiator comprises:
[0040] The multifunctional vinyl ester resin, active diluent and ultraviolet light initiator are mixed, ultrasonically treated and heated, and then degassed in a vacuum drying oven to obtain a matrix, wherein the heating temperature is 40-60°C; the ultrasonic treatment time is 20min-30min; the vacuum degree of the degassed process is -0.1 to -0.3MPa, and the treatment time is 20min-30min.
[0041] According to an embodiment of the present invention, the mass ratio of the multifunctional vinyl ester resin, the reactive diluent, and the ultraviolet light initiator is (20-40): (5-15): (0.5-2). The inventors found that if the reactive diluent content is too high, the viscosity of the resin system is significantly reduced, and the comprehensive performance of the product after curing is significantly reduced, which is not conducive to the high performance of the composite material. If the reactive diluent content is too low, there is a concentrated heat release phenomenon during the curing process, which leads to yellowing of the resin; if the photoinitiator content is too high, the absorption of ultraviolet light by the initiator during the photocuring process will cause its penetration depth to decrease, which is not conducive to the deep curing of the product. If the photoinitiator content is too low, the photocuring efficiency is reduced and the curing effect of the product is poor. Therefore, the photocurable resin matrix composed of the present application can be used to prepare glass fiber reinforced resin-based composite materials with excellent properties such as photocuring performance, mechanical properties, and heat resistance.
[0042] According to an embodiment of the present invention, the multifunctional vinyl ester resin includes at least one of bisphenol A epoxy acrylate, novolac epoxy acrylate, epoxidized oil acrylate and modified epoxy acrylate. The vinyl ester resin in the present invention has the following characteristics: ① It contains two or more highly active carbon-carbon double bond groups, which can participate in the free radical or cationic reaction of the photocuring process; ② It has one or more benzene ring rigid structures to improve the mechanical properties of the resin matrix. ③ It is liquid at room temperature and has appropriate viscosity, so it has excellent photocuring performance.
[0043] According to an embodiment of the present invention, the reactive diluent includes at least one of a monofunctional acrylate derivative such as 2-hydroxy-3-phenoxypropyl acrylate, a difunctional acrylate derivative such as 2-acrylate-2-hydroxy-1,3-propanediol, a multifunctional acrylate derivative such as trimethylolpropane triacrylate, and an acrylic acid modified compound. The reactive diluent in the present invention has the following characteristics: ① It has one or more highly active carbon-carbon double bond groups that can participate in free radical or cationic reactions in the photocuring process; ② It is liquid at room temperature, has a boiling point higher than 150°C, and has a lower viscosity than the selected resin, and can be used to adjust the photocuring performance of the system.
[0044] According to an embodiment of the present invention, the ultraviolet initiator includes at least one of acylphosphine oxides such as trimethylbenzoyl-diphenylphosphine oxide, benzophenones such as 2,4-dihydroxybenzophenone, and benzil types such as α,α-dimethoxy-α-phenylacetophenone. The ultraviolet initiator described in the present invention has the following characteristics: ① The near-ultraviolet light with a wavelength range of 320 to 400nm is optimal, and the larger the wavelength, the higher the penetration depth of the light source; ② The state at room temperature is solid or liquid, has good thermal stability, and has a certain solubility in vinyl ester resin; ③ Absorption of ultraviolet light can form free radicals or cationic active species, thereby initiating carbon-carbon double bond addition crosslinking.
[0045] Furthermore, in the process of mixing the multifunctional vinyl ester resin, the reactive diluent and the ultraviolet light initiator, an auxiliary agent may be added, and the auxiliary agent includes at least one of a toughening agent, a defoaming agent and an antioxidant. For example, the toughening agent includes but is not limited to styrene, polyolefin, polyester products and nanoparticles, etc., the defoaming agent includes but is not limited to silicone and polyether modified silicone oil defoaming agents, and the antioxidant includes but is not limited to hindered phenols and aromatic amine antioxidants.
[0046] S2: Using a winding device, the glass fiber bundle is impregnated with the matrix and then wound onto the mold.
[0047] Specifically, the program parameters that need to be modified are input into the operating software of the winding equipment (CNCFW-1-600 model), the trolley, boom and main shaft of the winding equipment are returned to the starting position and the equipment is put on standby, a unidirectional plate winding mold with a specification of 300mm*300mm*4mm is installed, the glass fiber spool is loaded and fixed, 300-500g of matrix is added to the resin tank, the glass fiber bundle is pulled and fixed to the mold, the winding program is started, and the glass fiber bundle is impregnated with the matrix and then wound onto the mold.
[0048] Furthermore, the winding program parameters include: the winding method is hoop winding, the number of winding layers is 2 to 4 layers, the forward distance of the tow is 40 to 200 mm, the step is 0.5 to 0.8 times the width of a single bundle of yarn, the winding tension is 0 to 100 N, and the winding rate is 10 to 40° / min. Therefore, through the controllable molding process parameters of the winding equipment, it is easier to achieve continuous, uniform, and precise production of long fiber products; at the same time, this molding method is easy to combine with light curing technology to prepare high-performance light-curing composite materials.
[0049] According to an embodiment of the present invention, the glass fiber includes continuous fibers with a bundle specification of 3K to 12K, and glass fiber types with different components can be selected according to product requirements, such as E-glass fiber, C-glass fiber, and high-strength glass fiber. The inventor found that the glass fiber bundle specification has a great influence on the design of the winding molding process. If the number of glass fiber bundles is less than 3K, on the one hand, the yarn sheet width of the bundle itself is small, and it is easy to form gaps between the bundles during the winding molding process. On the other hand, the fiber cannot withstand a certain degree of tension level, resulting in poor surface accuracy of the product, which will cause the comprehensive performance of the composite material to decrease significantly; if the number of glass fiber bundles is greater than 12K, on the one hand, the yarn sheet width of the bundle is too large, and the fiber is prone to yarn folding and hair winding after passing through multiple rollers of the equipment. On the other hand, the resin is not easy to fully infiltrate the large bundle fiber, resulting in uneven resin content between various parts of the product, large differences in the degree of curing after curing, and even defects caused by resin shrinkage, which is also not conducive to the high performance of composite products. Therefore, the preferred glass fiber specifications of the present application are used, which is conducive to the production process of the winding molding process and can effectively improve the production efficiency and comprehensive performance of the product.
[0050] According to an embodiment of the present invention, the matrix and the glass fiber bundle are prepared in a mass ratio of the multifunctional vinyl ester resin, the reactive diluent, the ultraviolet light initiator and the glass fiber bundle of (20-40):(5-15):(0.5-2):(30-50).
[0051] S3: Remove the wound sample obtained in step S2 from the mold and perform light curing
[0052] Specifically, the wound sample obtained in step S2 is removed from the mold and transferred to an ultraviolet lamp device for light curing to obtain a composite material.
[0053] Furthermore, the ultraviolet light wavelength range of the ultraviolet lamp device is 320-400nm; and / or the irradiation power of the ultraviolet lamp device is 100-200W; and / or the irradiation distance of the ultraviolet lamp device is 5-30cm; and / or the irradiation time of the ultraviolet lamp device is 1-2min; the ambient temperature of the photocuring process is 20-50°C.
[0054] Furthermore, before curing the wound sample, a transparent adhesive paper or a transparent glass plate is fixed on the surface of the sample in advance, so as to improve the surface quality of the product through surface processing.
[0055] The present invention provides a method for preparing a glass fiber reinforced resin-based composite material by winding molding and ultraviolet light curing. According to the method of the embodiment of the present invention, not only can the production efficiency of the glass fiber reinforced resin-based composite material be significantly improved and the energy consumption in the curing molding process be reduced, but also the high-precision and stable molding process effectively ensures the high performance of the product. Specifically, the Tg of the photocurable resin matrix in the composite material obtained by the present invention can reach 87.7°C, indicating that the resin matrix has good heat resistance and dimensional stability; the curing time of the glass fiber reinforced resin-based composite material obtained by the present invention is within 2 minutes, the tensile strength can reach 773MPa, and the tensile modulus can reach 23.14GPa, indicating that the composite unidirectional plate has excellent mechanical properties.
[0056] The second aspect of the present invention provides a glass fiber reinforced resin-based composite material, which is prepared by the method described in the first aspect. It should be noted that the above characteristics and advantages for preparing the stripped fiber reinforced resin-based composite material are also applicable to the glass fiber reinforced resin-based composite material, which will not be repeated here.
[0057] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments. The present invention may also have other various embodiments, and those skilled in the art may make various corresponding changes and deformations according to the present invention without departing from the spirit and essence of the present invention, but these corresponding changes and deformations shall all belong to the protection scope of the claims attached to the present invention.
[0058] Example 1
[0059] (1) Weigh 240 g of vinyl ester resin bisphenol A ethoxylated diacrylate, 60 g of active diluent diallyl terephthalate and 5 g of ultraviolet light initiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, mix the vinyl ester resin, the active diluent and the ultraviolet light initiator, heat to 60° C. with an ultrasonic oscillator and disperse for 30 min to promote uniform mixing, and evacuate to -0.2 MPa in a vacuum drying oven for degassing for 30 min to obtain the desired resin matrix.
[0060] (2) Design a winding molding program and set the following winding program parameters: the winding method is circumferential winding, the number of winding layers is 2 layers, the forward distance of the tow is 160 mm, the step is 1.5 mm, the winding tension is 0 N, and the winding rate is 40° / min. After the trolley, arm, and main shaft of the winding equipment return to the starting position, the equipment is on standby. A unidirectional plate winding mold with a specification of 300 mm*300 mm*4 mm is installed, the glass fiber spool is loaded and fixed, and the resin matrix prepared in step (1) is added to the resin tank. The 6K glass fiber tow with a yarn width of 2.35 mm is impregnated with the resin matrix, and the mass ratio of the yarn sheet is approximately glass fiber: resin matrix = 1:1. It is pulled and fixed to the mold, and the winding program is started.
[0061] (3) The unidirectional board winding mold was removed, and a layer of 2 mm thick transparent tempered glass plate was fixed on the surface of the obtained sample. The sample was then transferred to an ultraviolet lamp device and cured at room temperature using 160 W ultraviolet light for 2 min. The plate was cut and processed to obtain a glass fiber reinforced resin-based composite unidirectional board.
[0062] Example 2
[0063] (1) Weigh 210 g of vinyl ester resin bisphenol A ethoxylated diacrylate, 90 g of active diluent diallyl terephthalate and 5 g of ultraviolet light initiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, mix the vinyl ester resin, the active diluent and the ultraviolet light initiator, heat to 60° C. with an ultrasonic oscillator and disperse for 30 min to promote uniform mixing, and evacuate to -0.2 MPa in a vacuum drying oven for degassing for 30 min to obtain the desired resin matrix.
[0064] (2) Design a winding molding program and set the following winding program parameters: the winding method is circumferential winding, the number of winding layers is 2 layers, the forward distance of the tow is 160 mm, the step is 1.5 mm, the winding tension is 0 N, and the winding rate is 40° / min. After the trolley, arm, and main shaft of the winding equipment return to the starting position, the equipment is on standby. A unidirectional plate winding mold with a specification of 300 mm*300 mm*4 mm is installed, the glass fiber spool is loaded and fixed, and the resin matrix prepared in step (1) is added to the resin tank. The 6K glass fiber tow with a yarn width of 2.35 mm is impregnated with the resin matrix, and the mass ratio of the yarn sheet is approximately glass fiber: resin matrix = 1:1. It is pulled and fixed to the mold, and the winding program is started.
[0065] (3) The unidirectional board winding mold was removed, and a layer of 2 mm thick transparent tempered glass plate was fixed on the surface of the obtained sample. The sample was then transferred to an ultraviolet lamp device and cured at room temperature using 160 W ultraviolet light for 2 min. The plate was cut and processed to obtain a glass fiber reinforced resin-based composite unidirectional board.
[0066] Example 3
[0067] (1) Weigh 180 g of vinyl ester resin bisphenol A ethoxylated diacrylate, 120 g of active diluent diallyl terephthalate and 5 g of ultraviolet light initiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, mix the vinyl ester resin, the active diluent and the ultraviolet light initiator, heat to 60° C. with an ultrasonic oscillator and disperse for 30 min to promote uniform mixing, and evacuate to -0.2 MPa in a vacuum drying oven for degassing for 30 min to obtain the desired resin matrix.
[0068] (2) Design a winding molding program and set the following winding program parameters: the winding method is circumferential winding, the number of winding layers is 2 layers, the forward distance of the tow is 160 mm, the step is 1.5 mm, the winding tension is 0 N, and the winding rate is 40° / min. After the trolley, arm, and main shaft of the winding equipment return to the starting position, the equipment is on standby. A unidirectional plate winding mold with a specification of 300 mm*300 mm*4 mm is installed, the glass fiber spool is loaded and fixed, and the resin matrix prepared in step (1) is added to the resin tank. The 6K glass fiber tow with a yarn width of 2.35 mm is impregnated with the resin matrix, and the mass ratio of the yarn sheet is approximately glass fiber: resin matrix = 1:1. It is pulled and fixed to the mold, and the winding program is started.
[0069] (3) The unidirectional board winding mold was removed, and a layer of 2 mm thick transparent tempered glass plate was fixed on the surface of the obtained sample. The sample was then transferred to an ultraviolet lamp device and cured at room temperature using 160 W ultraviolet light for 2 min. The plate was cut and processed to obtain a glass fiber reinforced resin-based composite unidirectional board.
[0070] Example 4
[0071] (1) Weigh 210 g of vinyl ester resin bisphenol A ethoxylated diacrylate, 90 g of active diluent diallyl terephthalate and 5 g of ultraviolet light initiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, mix the vinyl ester resin, the active diluent and the ultraviolet light initiator, heat to 60° C. with an ultrasonic oscillator and disperse for 30 min to promote uniform mixing, and evacuate to -0.2 MPa in a vacuum drying oven for degassing for 30 min to obtain the desired resin matrix.
[0072] (2) Design a winding molding program and set the following winding program parameters: the winding method is circumferential winding, the number of winding layers is 2 layers, the forward distance of the tow is 160 mm, the step is 1 mm, the winding tension is 10 N, and the winding rate is 40° / min. After the trolley, arm, and main shaft of the winding equipment return to the starting position, the equipment is on standby. A unidirectional plate winding mold with a specification of 300 mm*300 mm*4 mm is installed, the glass fiber spool is loaded and fixed, and the resin matrix prepared in step (1) is added to the resin tank. The 6K glass fiber tow with a yarn width of 2.35 mm is impregnated with the resin matrix, and the mass ratio of the yarn sheet is approximately glass fiber: resin matrix = 1:1. It is pulled and fixed to the mold, and the winding program is started.
[0073] (3) The unidirectional board winding mold was removed, and a layer of 2 mm thick transparent tempered glass plate was fixed on the surface of the obtained sample. The sample was then transferred to an ultraviolet lamp device and cured at room temperature using 160 W ultraviolet light for 2 min. The plate was cut and processed to obtain a glass fiber reinforced resin-based composite unidirectional board.
[0074] Example 5
[0075] (1) Weigh 210 g of vinyl ester resin bisphenol A ethoxylated diacrylate, 90 g of active diluent diallyl terephthalate and 5 g of ultraviolet light initiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, mix the vinyl ester resin, the active diluent and the ultraviolet light initiator, heat to 60° C. with an ultrasonic oscillator and disperse for 30 min to promote uniform mixing, and evacuate to -0.2 MPa in a vacuum drying oven for degassing for 30 min to obtain the desired resin matrix.
[0076] (2) Design a winding molding program and set the following winding program parameters: the winding method is circumferential winding, the number of winding layers is 2 layers, the forward distance of the tow is 160 mm, the step is 1 mm, the winding tension is 30 N, and the winding rate is 40° / min. After the trolley, arm, and main shaft of the winding equipment return to the starting position, the equipment is on standby. A unidirectional plate winding mold with a specification of 300 mm*300 mm*4 mm is installed, the glass fiber spool is loaded and fixed, and the resin matrix prepared in step (1) is added to the resin tank. The 6K glass fiber tow with a yarn width of 2.35 mm is impregnated with the resin matrix, and the mass ratio of the yarn sheet is approximately glass fiber: resin matrix = 7:3. It is pulled and fixed to the mold, and the winding program is started.
[0077] (3) The unidirectional board winding mold was removed, and a layer of 2 mm thick transparent tempered glass plate was fixed on the surface of the obtained sample. The sample was then transferred to an ultraviolet lamp device and cured at room temperature using 160 W ultraviolet light for 2 min. The plate was cut and processed to obtain a glass fiber reinforced resin-based composite unidirectional board.
[0078] Example 6
[0079] (1) Weigh 210 g of vinyl ester resin bisphenol A ethoxylated diacrylate, 90 g of active diluent diallyl terephthalate and 5 g of ultraviolet light initiator diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, mix the vinyl ester resin, the active diluent and the ultraviolet light initiator, heat to 60° C. with an ultrasonic oscillator and disperse for 30 min to promote uniform mixing, and evacuate to -0.2 MPa in a vacuum drying oven for degassing for 30 min to obtain the desired resin matrix.
[0080] (2) Design a winding molding program and set the following winding program parameters: the winding method is hoop winding, the number of winding layers is 2 layers, the forward distance of the tow is 160 mm, the step is 1 mm, the winding tension is 50 N, and the winding rate is 40° / min. After the trolley, arm, and main shaft of the winding equipment return to the starting position, the equipment is on standby. A unidirectional plate winding mold with a specification of 300 mm*300 mm*4 mm is installed, the glass fiber spool is loaded and fixed, and the resin matrix prepared in step (1) is added to the resin tank. The 6K glass fiber tow with a yarn width of 2.35 mm is impregnated with the resin matrix, and the mass ratio of the yarn sheet is approximately glass fiber: resin matrix = 3:1. It is pulled and fixed to the mold, and the winding program is started.
[0081] (3) The unidirectional board winding mold was removed, and a layer of 2 mm thick transparent tempered glass plate was fixed on the surface of the obtained sample. The sample was then transferred to an ultraviolet lamp device and cured at room temperature using 160 W ultraviolet light for 2 min. The plate was cut and processed to obtain a glass fiber reinforced resin-based composite unidirectional board.
[0082] Performance Testing
[0083] 1. Composite material structure characterization: The mass and volume of resin, glass fiber and composite material are measured by measuring mass and volume, and the corresponding density is calculated.
[0084] m 复材 =m 树脂 +m 纤维
[0085] V 复材 =V 树脂 +V 纤维 +V 孔隙
[0086] Fiber% = 100% * V 纤维 / V 复材 , Porosity% = 100*V 孔隙 / V 复材For the resin matrix and composite material specimens, the mass was weighed with a balance, and the volume was measured by immersing the sample in a measuring cylinder filled with deionized water to calculate the density; for glass fiber, its bulk density was measured by a density gradient meter, and a certain mass of composite material was calcined at 600℃ for 30min in a muffle furnace, and the fiber mass was weighed after cooling to calculate its volume. The mass of the pores was ignored, and its volume ratio was calculated.
[0087] 2. Mechanical properties test: According to GB / T 3354-2014, the glass fiber reinforced resin-based composite unidirectional plates prepared in Examples 1-6 were cut into 250mm*12.5mm*2mm tensile specimens, and 50mm*12.5mm*1mm non-woven fabric reinforced composite reinforcement sheets were pasted on both ends, with no less than 5 specimens per group. An Instron 6800 universal material testing machine was used to continuously load the samples at a speed of 2mm / min at room temperature, and the load-strain results of the samples were recorded. The tensile strength and tensile modulus were calculated as the mechanical properties of the products.
[0088]
[0089] Where, σ is the tensile strength of the sample, in MPa; P max ——The maximum load that the specimen can withstand before failure, in N; w——The width of the specimen, in mm; h——The thickness of the specimen, in mm.
[0090]
[0091] Where, E is the tensile modulus of the specimen, in GPa; Δσ is the increment of the tensile strength of the specimen within the longitudinal strain range of 0.001 to 0.003, in MPa; Δε is the strain increment of the specimen within the longitudinal strain range of 0.001 to 0.003, in mm / mm.
[0092] The above test results are shown in Table 1.
[0093] Table 1 Structural properties of glass fiber reinforced resin-based composite one-way plates prepared in various embodiments of the present invention
[0094]
[0095]
[0096] From the results in Table 1, it can be seen that in Examples 1-3 of the present invention, as the content of the active diluent increases, the viscosity of the resin system decreases significantly, and the comprehensive performance of the product after curing decreases significantly, which is not conducive to the high performance of the composite material. The fiber volume fraction and pore volume fraction do not change much, but the tensile strength and tensile modulus gradually decrease. In Examples 4-6 of the present invention, as the winding tension gradually increases, more resin is scraped out after the fiber passes through the roller, so that the fiber volume content of the composite product is higher, and the fibers are arranged more closely to each other, thereby giving the composite material a more complete structure and performance.
[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a glass fiber reinforced resin-based composite material, characterized in that: include: (1) mixing a multifunctional vinyl ester resin, a reactive diluent and an ultraviolet light initiator to prepare a matrix; (2) using a winding device to impregnate the glass fiber bundle with the substrate and then wind it onto the mold; (3) removing the wound sample obtained in step (2) from the mold and performing photocuring to obtain a composite material.
2. The method according to claim 1, characterized in that The mass ratio of the multifunctional vinyl ester resin, the reactive diluent, the ultraviolet light initiator and the glass fiber bundle is (20-40): (5-15): (0.5-2): (30-50).
3. The method according to claim 1 or 2, characterized in that: In step (1), the multifunctional vinyl ester resin, reactive diluent and ultraviolet light initiator are mixed to prepare a matrix comprising: The multifunctional vinyl ester resin, the active diluent and the ultraviolet light initiator are mixed, subjected to ultrasonic treatment and heating, and then degassed in a vacuum drying oven to obtain a matrix; Optionally, the heating temperature is 40-60°C; Optionally, the ultrasonic treatment time is 20min-30min; Optionally, the vacuum degree of the degassing process is -0.1 to -0.3 MPa, and the processing time is 20 min to 30 min.
4. The method according to claim 1 or 2, characterized in that: In step (1), an auxiliary agent may be added during the mixing of the multifunctional vinyl ester resin, the reactive diluent and the ultraviolet light initiator. The auxiliary agent includes at least one of a toughening agent, a defoaming agent and an antioxidant.
5. The composite material according to claim 1 or 2, characterized in that: In step (1), the multifunctional vinyl ester resin includes at least one of bisphenol A epoxy acrylate, novolac epoxy acrylate, epoxidized oil acrylate and modified epoxy acrylate.
6. The composite material according to claim 1 or 2, characterized in that: In step (1), the reactive diluent includes at least one of a monofunctional acrylate derivative, a difunctional acrylate derivative, and a multifunctional acrylate derivative; Optionally, in step (1), the ultraviolet light initiator comprises at least one of acylphosphine oxides, benzophenone compounds and benzil compounds.
7. The composite material according to claim 1 or 2, characterized in that: In step (2), the glass fiber bundle includes at least one of E-glass fiber, C-glass fiber and high-strength glass fiber.
8. The method according to claim 1 or 2, characterized in that: In step (2), the parameters of the winding device include at least one of the following: The winding method of the winding device is hoop winding; The number of winding layers of the glass fiber bundle is 2 to 4; The advancing distance of the glass fiber bundle is 40 to 200 mm; The stepping of the glass fiber bundle is 0.5 to 0.8 times the width of a single bundle yarn sheet; The winding tension of the glass fiber bundle is 0 to 100N; The winding rate of the glass fiber bundle is 10-40° / min.
9. The method according to claim 1 or 2, characterized in that: In step (3), the photocuring comprises: The wound sample obtained in step (2) is removed from the mold and transferred to a UV lamp device for light curing; Optionally, before curing the wound sample, a transparent adhesive paper or a transparent glass plate is fixed on the surface of the sample in advance; Optionally, the ultraviolet light wavelength range of the ultraviolet lamp device is 320-400nm; and / or the irradiation power of the ultraviolet lamp device is 100-200W; and / or the irradiation distance of the ultraviolet lamp device is 5-30cm; and / or the irradiation time of the ultraviolet lamp device is 1-2min; the ambient temperature of the photocuring process is 20-50°C.
10. A glass fiber reinforced resin-based composite material, characterized in that: The method according to any one of claims 1 to 9 is used to prepare the present invention.
Citation Information
Patent Citations
Method for producing pressure vessel
EP2740584A1