Polyester resin composition and molded article for capacitor housing produced using same
By using a polyester resin composition in a capacitor housing, it includes polybutylene terephthalate, acrylic-styrene-acrylonitrile resin, glass fiber, epoxy resin, carbodiimine-based anti-hydrolyzer and Epoxy silane solves the problems of insufficient adhesion and poor hydrolysis resistance of polybutylene terephthalate-based materials, achieves high adhesion and dimensional stability, and maintains good conditions under high temperature and high humidity environments. performance.
Patent Information
- Application Number
- CN202410629794.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-03
AI Technical Summary
The existing polybutylene terephthalate-based materials have problems such as insufficient adhesion, poor hydrolysis resistance and difficulty in ensuring high dimensional stability in the capacitor housing, especially when using epoxy potting materials.
Polyester resin composition is used, which contains 40-50% polybutylene terephthalate resin, 18-20% acrylic-styrene-acrylonitrile resin, 25-35% glass fiber, 1- 3% epoxy resin, 0.01-1% carbodiimide anti-hydrolyzer and 0.01-1% epoxy silane, through the combination of these components, the adhesion and dimensional stability are improved, and at high temperatures. Maintain good performance in wet environments.
The high adhesion, dimensional stability and hydrolysis resistance of the capacitor housing are achieved, ensuring long-term reliability in harsh environments and reducing manufacturing costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 2023-0069690, filed on May 31, 2023, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] The present invention relates to a polyester resin composition and a capacitor case molded product manufactured using the same, and more particularly to a polyester resin composition having excellent adhesion to an epoxy potting material and being able to simultaneously satisfy dimensional stability and hydrolysis resistance, and a capacitor case molded product manufactured using the polyester resin composition. Background Art
[0004] The DC capacitor is a key part of the H(E)PCU module and is the part that eliminates DC voltage pulsation (has a smoothing function). Conventionally, the capacitor case material is made by mixing a polyphenylene sulfide (PPS)-based resin with a high content of filler, but attempts have been made to make alternative products using more economical polyester resins.
[0005] Capacitor manufacturing often involves injecting epoxy potting materials. Potting is a method of encapsulating electronic components such as devices by covering them with plastic resin. Liquid resin is injected into the housing where the device is placed, or viscous resin is dripped directly onto the device and hardened. This method is widely used due to its simplicity and flexibility in resin selection.
[0006] Epoxy potting materials are also used to manufacture DC inverter capacitors, such as the present invention. Therefore, the adhesion of the capacitor housing to the epoxy potting material is important. In other words, the capacitor housing must ensure a high level of bonding strength and strength retention with the molding liquid (epoxy resin) to protect the capacitor from internal moisture and ensure insulation. However, in the case of polybutylene terephthalate (PBT)-based materials, there are limitations on improving epoxy resin adhesion, poor hydrolysis resistance, and difficulty in ensuring high dimensional stability. In addition, since the viscosity of polybutylene terephthalate (PBT) resin is higher than that of polyphenylene sulfide (PPS) resin, there are problems in ensuring high dimensional stability by specifying a large amount of minerals, making it difficult to include a high content of filler.
[0007] Therefore, it is necessary to develop a polyester resin composition for capacitor cases which has excellent adhesion to epoxy potting materials and also has excellent dimensional stability and hydrolysis resistance. Summary of the invention
[0008] The present disclosure aims to provide a polyester resin composition having high dimensional stability, excellent adhesion to an epoxy potting agent, and excellent hydrolysis resistance, and a molded article for a capacitor case produced by molding the polyester resin composition.
[0009] In order to solve the above technical problems, as an embodiment of the present invention, a polyester resin composition for a capacitor case is provided, which comprises, based on the total weight of the polyester resin composition, 40 to 50 weight % of polybutylene terephthalate resin; 18 to 20 weight % of acrylic-styrene-acrylonitrile resin; 25 to 35 weight % of glass fiber; 1 to 3 weight % of epoxy resin; 0.01 to 1 weight % of carbodiimide anti-hydrolysis agent; and 0.01 to 1 weight % of epoxy silane.
[0010] In one embodiment, the polybutylene terephthalate resin may have an intrinsic viscosity of 0.80 to 1.00 dl / g.
[0011] In one embodiment, the rubber content of the acrylic-styrene-acrylonitrile resin may be 20 to 60 parts by weight.
[0012] In one embodiment, the glass fiber may be a flat glass fiber having an average diameter of 30 to 40 μm and a length of 3 to 4 mm.
[0013] As another embodiment of the present invention, a molded article for a capacitor case including a polyester resin composition is provided.
[0014] In one embodiment, the average linear expansion coefficient of the molded article measured by the ISO 11359 test method can be 50×10 -6 / ℃ to 55×10 -6 / ℃ range.
[0015] In one embodiment, the initial adhesive strength measured by the ISO 4587 test method may be in the range of 3.0 to 3.5 MPa.
[0016] In one embodiment, the adhesive strength of the molded article measured after 1000 hours under environmental conditions of a temperature of 85° C. and a relative humidity of 85% may be 94% or more of the initial adhesive strength.
[0017] In one embodiment, the adhesive strength of the molded article measured after 96 hours under environmental conditions of a temperature of 120° C. and a relative humidity of 100% may be 75% or more of the initial adhesive strength.
[0018] In one embodiment, the relative tracking index (CTI) grade of the molded article can be in the range of 0 to 2, and the grade of 0 to 2 can be maintained even after 1000 hours under environmental conditions of a temperature of 85° C. and a relative humidity of 85% or after 96 hours under environmental conditions of a temperature of 120° C. and a relative humidity of 100%. DETAILED DESCRIPTION
[0019] Hereinafter, the present invention will be described in more detail with reference to embodiments. However, the following embodiments are provided by way of example to help understand the present invention, and the scope of the present invention is not limited thereto. It should be understood that the present invention includes various modifications and can be implemented in many different forms, and all modifications, equivalents and substitutes are included in the spirit and scope of the present invention.
[0020] The terms used in this application are only used to describe specific embodiments and are not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly stipulates otherwise. In this application, it should be understood that the terms "including" or "having" etc. are intended to specify the existence of stated features, numbers, steps, operations, components, parts or combinations thereof, but do not exclude the existence or addition of one or more other features, numbers, steps, operations, components, parts and combinations thereof.
[0021] Unless otherwise defined, all terms (including technical or scientific terms) used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an idealized or overly formal sense unless clearly defined in this application.
[0022] The polyester resin composition for capacitor case of the embodiment of the present invention comprises polybutylene terephthalate (PBT) resin and acrylic-styrene-acrylonitrile (ASA) resin as base resin, glass fiber as filler, and epoxy resin, anti-hydrolysis agent and epoxy silane as additives. The detailed description of each component and material is as follows.
[0023] Polybutylene terephthalate
[0024] The polyester resin composition according to the embodiment includes polybutylene terephthalate (PBT) as a crystalline base resin. Polybutylene terephthalate (PBT) resin refers to polybutylene terephthalate homopolymer and polybutylene terephthalate copolymer. Polybutylene terephthalate resin can be manufactured by direct esterification of 1,4-butanediol and terephthalic acid or dimethyl terephthalate, or by transesterification and polycondensation.
[0025] In addition, for the impact strength and surface modification of the polybutylene terephthalate resin, a copolymer obtained by copolymerizing a polybutylene terephthalate polymer with components such as polytetramethylene glycol (PTMG), polyethylene glycol (PEG), polypropylene glycol (PPG), aliphatic polyester, and aliphatic polyamide, or a modified polybutylene terephthalate resin as a blended composition blended with these components may also be used.
[0026] The intrinsic viscosity (η) of the polybutylene terephthalate resin that can be used in the polyester resin composition according to the embodiment measured according to ASTM D2857 can be 0.80dl / g to 1.00dl / g. When the intrinsic viscosity of polybutylene terephthalate (PBT) resin is less than 0.80dl / g, it may be difficult to ensure mechanical properties, and as the flow index of the material increases, the bending characteristics of the injection molded product may increase, or the appearance of burrs may increase, resulting in unnecessary post-processing. When the intrinsic viscosity exceeds 1.00dl / g, the flow index may decrease, which may cause the surface quality of the injection molded product to deteriorate and the molding processability to decrease. When the intrinsic viscosity of the polybutylene terephthalate resin is within the above range, the polyester resin composition comprising the resin can ensure fluidity, and therefore can ensure the moldability (moldability) of large molded products with complex structures.
[0027] The polyester resin composition for capacitor housing may include 40 to 50 wt % of polybutylene terephthalate (PBT) resin based on the total weight of the resin composition. When the content of the polybutylene terephthalate (PBT) resin is less than 40 wt %, there is a problem of reduced mechanical strength, and when the content of the polybutylene terephthalate (PBT) resin exceeds 50 wt %, the dimensional stability of the injection molded product may be reduced.
[0028] Compared with other resins, polybutylene terephthalate has excellent overall physical properties such as fluidity and surface smoothness, and has excellent moldability for complex structures. In addition, compared with the case of using polybutylene terephthalate resin mixed with other polyester resins, excellent physical properties can be ensured.
[0029] Acrylonitrile-styrene-acrylate
[0030] The polyester resin composition according to an embodiment includes an acrylonitrile-styrene-acrylate (ASA) copolymer as an amorphous base resin.
[0031] Acrylonitrile-styrene-acrylate (ASA) copolymer is a terpolymer of styrene, acrylonitrile and acrylate rubber. Acrylonitrile-styrene-acrylate (ASA) copolymer can be a graft blend type copolymer, and the acrylate rubber can be copolymerized in a ratio of 20 to 60 weight % based on the total weight of the copolymer. When the ratio of the acrylate rubber included in the ASA copolymer is less than 20 weight %, the impact strength of the entire resin may be reduced, and when the ratio exceeds 50 weight %, the tensile strength and heat distortion temperature (HDT) may be reduced due to the increase of the flow index.
[0032] When acrylonitrile-styrene-acrylate is included in the polyester resin composition, the effects of improving the specific gravity, dimensional stability, heat resistance stability and weather resistance of the resin composition can be obtained. In addition, the polyester resin composition can maintain glossiness and has excellent molding processability due to the inclusion of acrylonitrile-styrene-acrylate (ASA) resin, which has the advantage that it can be applied to various molding methods such as injection, extrusion and calendaring.
[0033] The polyester resin composition for capacitor housing may include 18 to 20 wt % of acrylonitrile-styrene-acrylate (ASA) copolymer based on the total weight of the resin composition. When the content of acrylonitrile-styrene-acrylate (ASA) copolymer is less than 18 parts by weight, the dimensional stability effect cannot be achieved, and when the content of acrylonitrile-styrene-acrylate (ASA) copolymer exceeds 20 parts by weight, the crystallization temperature of the material may decrease, which may result in poor injection molding release and reduced mechanical strength and heat deformation temperature (HDT) of the molded body.
[0034] filler
[0035] In the polyester resin composition according to the embodiment, flat glass fibers are used as fillers. The glass fibers that can be used may have an average diameter of 30 to 40 μm and a length of 3 to 4 mm. Using flat glass fibers within the above range can improve the dimensional stability of the molded product by improving the GF bias.
[0036] The flat glass fiber used as a filler can be used in an amount of 10 to 30% by weight based on the entire polyester resin composition for capacitor cases. When the filler content is less than the above range, there are problems such as reduced mechanical strength, increased bending characteristics of injection molded products, and reduced dimensional stability, and when the content exceeds the above range, mechanical properties are improved, but there is a problem of poor processability due to reduced molding shrinkage.
[0037] Epoxy resin
[0038] The epoxy resin according to the embodiment may be a solid bisphenol A epoxy resin having a medium molecular weight level.
[0039] The bisphenol A epoxy resin reacts with the ethylene backbone of the polybutylene terephthalate (PBT) base resin to form a bond, thereby enhancing adhesion to the epoxy resin and improving hydrolysis resistance. For example, a bisphenol A epoxy resin having an epoxy equivalent weight (EEW) in the range of 900 to 1,950 g / eq may be used.
[0040] The epoxy resin used as an additive may be used in a range of 1 wt % to 3 wt % based on the entire polyester resin composition for capacitor cases. When the content of the epoxy resin is less than the above range, there is a problem that adhesion to the epoxy resin and hydrolysis resistance may be reduced, and when the content exceeds the above range, there is a problem that mechanical properties may be reduced.
[0041] Anti-hydrolysis agent
[0042] The polyester resin composition according to an embodiment may have improved hydrolysis stability by introducing an additive having a carbodiimide bond for end-capping.
[0043] The carbodiimide compound useful as an anti-hydrolysis agent may be a monomer type or a polymer type, and a combination of a monomer type and a polymer type may be used according to the purpose of use of the resin composition. In the monomer type, one molecule of the carbodiimide compound reacts with an end group of the polyester to provide hydrolysis resistance, and in the polymer type, an end group of the carbodiimide compound reacts with an end group of the polyester.
[0044] Specific examples of carbodiimide compounds include N,N'-di-o-tolylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-dioctyldecylcarbodiimide, N,N'-di-2,6-diketylphenylcarbodiimide, N-tolyl-N'-cyclohexylcarbodiimide, N,N'-di-2,6-diisopropylphenylcarbodiimide, N,N'-di-2,6-di-tert-butylphenylcarbodiimide, N-tolyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N '-Di-p-hydroxyphenylcarbodiimide, N,N'-dicyclohexylcarbodiimide, N,N'-di-p-tolylcarbodiimide, p-phenylene-bis-di-o-tolylcarbodiimide, p-phenylene-bis-dicyclohexylcarbodiimide, hexamethylene-bis-dicyclohexylcarbodiimide, ethylene-bis-diphenylcarbodiimide, benzene-2,4-diisocyanato-1,3,5-tri(1-methylethyl) homopolymer, and a copolymer of 2,4-diisocyanato-1,3,5-tri(1-methylethyl) and 2,6-diisopropyl diisocyanate, one or more of which can be selected and used as the anti-hydrolysis agent.
[0045] The anti-hydrolysis agent may be used in an amount of 0.01 wt % to 1 wt % based on the entire polyester resin composition for capacitor cases. When the content of the anti-hydrolysis agent is less than the above range, the effect of inhibiting hydrolysis is minimal, and when the content exceeds the above range, the physical properties of the resin composition may be affected without further improving hydrolysis resistance.
[0046] Epoxy silane
[0047] In order to improve adhesion with an epoxy potting material used to manufacture a capacitor case, the polyester resin composition according to an embodiment may include epoxy silane as an additive.
[0048] The epoxysilane used as the additive may be a silane coupling agent having an epoxy group or a glycidyl group, and may include 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-glycidoxypropyltriethoxysilane, etc., wherein one or more may be selected and used.
[0049] The epoxy silane used as an additive may be used in the range of 0.01 wt % to 1 wt % based on the entire polyester resin composition for capacitor cases. When the content of the epoxy silane is less than the above range, the effect of improving the adhesion with the epoxy potting material is minimal, and when the content exceeds the above range, the viscosity of the material increases, which may cause problems in injection processability and surface quality of injection molded products.
[0050] Example 1: Preparation of polyester resin composition
[0051] In order to prepare the resin composition for a capacitor case, a polybutylene terephthalate (PBT) resin is prepared as a crystalline base resin, and an acrylic styrene acrylate (ASA) resin is prepared as an amorphous base resin to improve dimensional stability, as follows.
[0052] [Table 1]
[0053] Classification grade supplier characteristic Remark PBT 1200-211M CHANG CHUN IV 0.83 ASA LI912 LG CHEM MI 12 220℃,10kg
[0054] In addition, the GF deviation is improved by using flat glass fibers as fillers, thereby improving dimensional stability.
[0055] [Table 2]
[0056]
[0057] In addition, epoxy resin, epoxy silane and anti-hydrolysis agent are used as additives. Epoxy resin and epoxy silane are used to increase the adhesion with epoxy potting materials used to manufacture capacitor cases and improve hydrolysis performance.
[0058] In addition, carbodiimide compounds are used as anti-hydrolysis agents to improve the hydrolysis performance of the capacitor shell.
[0059] [Table 3]
[0060]
[0061] Using the materials prepared above, each material was uniformly mixed according to the weight percentage shown in Table 4 below to prepare a resin composition.
[0062] [Table 4]
[0063]
[0064] Comparative Example 1
[0065] The resin composition for a capacitor case is prepared using a modified polyphenylene ether (MPPO)-based resin instead of PBT as a base resin.
[0066] Comparative Example 2
[0067] The resin composition for capacitor cases was prepared without using an anti-hydrolysis additive.
[0068] Test Example 1: Physical property evaluation of molded products
[0069] Molded articles were manufactured using the polyester resin composition prepared in Example 1 and the resin compositions of Comparative Examples 1 and 2, and the linear expansion coefficient, flexural strength, and flexural modulus were measured, and the test results are listed in Table 5 below.
[0070] The coefficient of linear expansion is measured under ISO 11359 conditions in the temperature range of -40 to 110°C.
[0071] [Table 5]
[0072]
[0073] Test Example 2: Evaluation of epoxy resin adhesion
[0074] Molded articles were manufactured using the polyester resin composition prepared in Example 1 and the resin compositions of Comparative Examples 1 and 2, and the epoxy resin adhesion was evaluated under severe durability conditions, and the test results are listed in Table 6 below.
[0075] [Table 6]
[0076]
[0077] Test Example 3: Insulation (withstand voltage) evaluation
[0078] Molded articles were made using the polyester resin composition prepared in Example 1 and the resin compositions of Comparative Examples 1 and 2, and the hydrolysis resistance was evaluated by measuring changes in physical properties after being placed in a high temperature / high humidity environment for a long time. Specifically, the flexural strength, flexural modulus, and insulation (CTI, withstand voltage) were measured after 1000 hours in an 85°C / 85% RH environment.
[0079] - Flexural strength: According to the evaluation method specified in ISO 178, the specimen size is 80×10×4 mm, the span length is 64 mm, the test speed is 2 mm / min, and the unit is MPa.
[0080] -Flexural modulus: According to the evaluation method specified in ISO 178, the specimen size is 80×10×4 mm, the span length is 64 mm, the test speed is 2 mm / min, and the unit is MPa.
[0081] - Withstand voltage verification: Verify insulation breakdown at the start and after being placed at 3kV for 1 minute after high temperature / high humidity.
[0082] [Table 7]
[0083]
[0084] As a result of checking the physical property change rate of the polyester resin composition of Example 1, the bending property retention rate of the material to be evaluated after environmental reliability was 93% or more, maintaining the same level as the initial level. By adding a carbodiimide compound for ensuring hydrolysis resistance, it was confirmed that hydrolysis resistance was improved and physical properties were maintained.
[0085] In addition, as a result of comparative tracking index (CTI) verification, the performance level category (PLC) of the polyester resin composition of Example 1 was measured as level 1, from which it can be seen that the insulation performance before and after the environmental reliability test is also excellent.
[0086] The capacitor case manufactured by molding the polyester resin composition of the present invention has high epoxy resin adhesion, excellent dimensional stability and hydrolysis resistance, and can also reduce manufacturing costs.
[0087] Specifically, the capacitor case molded article using the polyester resin composition of the embodiment of the present invention has high initial bond strength with epoxy resin, low change rate of bond strength even in a long-term high temperature and high humidity environment, and exhibits mechanical properties sufficient for use as a capacitor case.
[0088] Meanwhile, the effects of the present invention are not limited to the above-mentioned effects, and other effects that are not mentioned will be clearly understood by those skilled in the art from the above description.
Claims
1. A polyester resin composition for a capacitor housing, comprising, based on the total weight of the polyester resin composition: 40 to 50 wt% polybutylene terephthalate resin; 18 to 20 wt% acrylic-styrene-acrylonitrile resin; 25 to 35% by weight of glass fibers; 1 to 3 wt % epoxy resin; 0.01 to 1% by weight of a carbodiimide anti-hydrolysis agent; and 0.01 to 1 wt% epoxy silane.
2. The composition according to claim 1, wherein The polybutylene terephthalate resin has an intrinsic viscosity of 0.80 to 1.00 dl / g.
3. The composition according to claim 1, wherein The acrylic-styrene-acrylonitrile resin has a rubber content of 20 to 60%.
4. The composition according to claim 1, wherein The glass fibers are flat glass fibers having an average diameter of 30 to 40 μm and a length of 3 to 4 mm. 5 . A molded article for a capacitor case, comprising the polyester resin composition according to claim 1 .
6. The molded article according to claim 5, wherein The average linear expansion coefficient of the molded product measured by the ISO 11359 test method is 50×10 -6 / ℃ to 55×10 -6 / ℃ range.
7. The molded article according to claim 5, wherein The initial bonding strength of the molded article measured by ISO 4587 test method is in the range of 3.0 to 3.5 MPa.
8. The molded article according to claim 5, wherein The adhesive strength of the molded article measured after 1000 hours under environmental conditions of a temperature of 85° C. and a relative humidity of 85% is 94% or more of the initial adhesive strength.
9. The molded article according to claim 5, wherein The adhesive strength of the molded article measured after 96 hours under environmental conditions of a temperature of 120° C. and a relative humidity of 100% is 75% or more of the initial adhesive strength.
10. The molded article according to claim 5, wherein The comparative tracking index (CTI) grade of the molded article is in the range of 0 to 2.