Supercritical foaming PLA material and preparation method thereof
Through the supercritical foaming method and specific chemical combination, the problems of low melt strength of PLA and low solubility of foaming agents are solved, and PLA foam materials with high foaming ratio and cell uniformity are achieved, which improves the melt strength of PLA and Foaming properties maintain the degradability of the material.
Patent Information
- Application Number
- CN202411342235.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-03
AI Technical Summary
Polylactic acid (PLA) has low melt strength and low foaming agent solubility, resulting in low foaming ratio of PLA foam materials, cell collapse and unevenness.
Using supercritical foaming method, high-quality levopolylactic acid and specific peroxide initiator and chain extender are combined, and processed through a twin-screw extruder and flat vulcanizer, combined with supercritical CO2 foaming, optimize the process parameters to Improve the melt strength and foaming ratio of PLA.
The PLA foam material with high foaming ratio and cell uniformity is achieved, which improves the melt strength and foaming performance of PLA, maintains the degradability of the material, and prevents cell collapse at high foaming ratio.
Smart Images

Figure SMS_4 
Figure SMS_5 
Figure HDA0005060030550000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biodegradable polymer materials, and in particular relates to a supercritical foaming PLA material and a preparation method thereof. Background Art
[0002] Traditional petroleum-based plastics are a type of plastic material made from fossil fuels such as petroleum. They have good plasticity and mechanical properties and are widely used in various fields. The raw materials of traditional polymer materials mostly come from petroleum, such as polyethylene (PE), polypropylene (PP), and polyvinyl chloride (PVC). With the widespread use of traditional plastic products, the environmental problems they bring are becoming increasingly serious. At the same time, petroleum as a non-renewable resource is decreasing.
[0003] Polylactic acid (PLA) is a new type of environmentally friendly material with good performance. It is made by polymerizing lactic acid molecules. Lactic acid is fermented from starch and sugars in wheat, corn, grains, straw, etc. PLA is a renewable material with biodegradability. It can be naturally degraded in the natural environment. The final products of decomposition are water and carbon dioxide, which will not cause any pollution to the environment. PLA foaming materials have basically similar physical properties to petroleum-based foam plastics. They also have their own excellent characteristics and can be widely used in packaging and bio-consumer products. With the trend of replacing petroleum-based foam plastics, due to its superior performance and good application prospects, PLA foam plastics are increasingly becoming the first choice to replace traditional petroleum-derived polymer foam plastics that are currently widely used in packaging.
[0004] Supercritical foaming is an environmentally friendly physical foaming method. This method dissolves the physical foaming agent into PLA by pressurizing, and then uses pressure or temperature changes to promote the separation of the foaming agent from the matrix to form a pore structure. Currently, supercritical foaming has been widely used to produce various lightweight plastic foams. However, PLA has low melt strength and a narrow processing window for conventional methods, making it difficult to prepare PLA foam materials with high foaming ratios and small pore diameters.
[0005] Patent CN114989589A discloses a high-expansion PLA foam and a preparation method thereof. The method improves the expandability of PLA by adding a chain extender and polytetrafluoroethylene (PTFE), thereby obtaining a PLA foam material with a low cell size and a high cell density, but the maximum expansion ratio of the invention is only 12.
[0006] CN112920583A discloses a fast-crystallizing poly-L-lactic acid foam material and a preparation method thereof. The method adds PLLA-b-PDLA block copolymer and nano bubble nucleating agent, and adopts injection molding process to obtain a heat-resistant, stable foaming, and high-density PLA foam material, with an average foaming ratio of about 30. CN115746524A discloses a biodegradable micro-foamed PLA material and a preparation method thereof. The method combines the synthesized polybenzidine-pyridine-benzimidazole with a bio-polyester resin, an initiator, an antioxidant, a multifunctional monomer, etc., and the micro-foamed PLA material obtained by extrusion has an overall density of 400kg / m 3 ~600kg / m 3 between. Summary of the invention
[0007] In view of the defects of polylactic acid (PLA) pointed out in the background technology, such as low melt strength and low solubility of foaming agent, and the problems of low foaming ratio, cell collapse and unevenness of PLA foam material after foaming, the present invention aims to provide a method for preparing a supercritical foaming PLA material with high foaming ratio and uniform cells.
[0008] In order to achieve the above object, the present invention adopts the following technical scheme:
[0009] A supercritical foamed PLA material, comprising the following components by mass fraction
[0010] PLA 95.25%~99.25%;
[0011] Peroxide initiator 0.25% to 0.75%;
[0012] Chain extender 0.5% to 4%;
[0013] Furthermore, the PLA is L-polylactic acid with an optical purity greater than 85% and a density of 1.24 g / cm 3 Preferably, PLA is L-polylactic acid with an optical purity of >88%, such as Total Energy Cobien LX975; or L-polylactic acid with an optical purity greater than 96%, such as LX175; or L-polylactic acid with an optical purity of >98%, 99%, such as LX575, L175, etc.
[0014] Further, the peroxide initiator is one or more combinations of 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-nonane peroxide, di-tert-butyl peroxide (DTBP), tert-amyl peroxide pivalate, and diisopropyl peroxydicarbonate. The preferred peroxide initiator is 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane.
[0015] Furthermore, the chain extender is a diepoxy functional group-containing auxiliary agent, including any one of 1,6-hexanediol diglycidyl ether, 1,3-diepoxyglyceryl ether glycerol, diglycidyl ether, 1,4-bis(oxidized glycidyl)benzene, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, and bisphenol A diglycidyl ether, or a mixture of any two or more thereof in any ratio.
[0016] The preparation method of the supercritical foamed PLA material comprises the following steps:
[0017] Step (1): weighing PLA, peroxide initiator, and chain extender according to mass fraction;
[0018] Step (2): placing the components weighed in step (1) in a low-speed mixer and blending them to obtain a mixed material;
[0019] Step (3): drying the mixture obtained in step (2) and adding it to a twin-screw extruder for extrusion and granulation to obtain LCB-PLA particles;
[0020] Step (4): drying the LCB-PLA particles obtained in step (3) and then subjecting the particles to a flat vulcanizing machine to obtain a sheet;
[0021] Step (5): placing the sheet obtained in step (4) into a supercritical foaming reactor, heating it to a foaming temperature, introducing a physical foaming agent into the reactor, foaming, and rapidly releasing the pressure to obtain a PLA foamed material;
[0022] Furthermore, the mixing time in the low-speed mixer in step (2) is 20 min to 30 min.
[0023] Furthermore, in step (3), the drying treatment temperature is 60° C. to 80° C., and the drying time is 2 h to 6 h.
[0024] Furthermore, in step (3), the screw temperature of the twin-screw extruder from the feed section to the die is set to 140°C to 190°C (lower than the temperature required for the reaction of hydroxyl groups and epoxy groups in PLA); the twin-screw extruder is divided into five parts: forward conveying, mixing, reverse conveying, secondary forward conveying, and die, wherein the temperature of the forward conveying part is 140°C to 180°C, the temperature of the mixing and reverse conveying parts is both 180°C, and the temperature from the secondary forward conveying part to the die is gradually increased from 180°C to 190°C; the screw aspect ratio of the twin-screw extruder is above 64:1, and the screw speed is 50rpm to 400rpm.
[0025] Furthermore, the drying treatment temperature in step (4) is 60°C to 80°C, and the drying time is 2h to 6h; the temperature of the flat vulcanizing press in step (4) is 180°C.
[0026] Furthermore, the physical foaming agent in step (5) is supercritical CO2 with a purity of 99.9%.
[0027] Furthermore, in step (5), the foaming temperature is 115° C. to 135° C.; the foaming fluid pressure is 5 MPa to 15 MPa; and the saturation time is 0.5 h to 2 h.
[0028] Furthermore, the pressure relief time in step (5) is 2s, and the kettle can be opened and the material can be discharged after the pressure is reduced to normal pressure.
[0029] The beneficial effects of the present invention are:
[0030] First, the present invention preferably uses peroxide initiator to reduce the recombination reaction of PLA macromolecular free radicals, so that the PLA macromolecular reaction tends to undergo chain transfer reaction, and long branch chains are added to other long branch chains to form a branch-branch-branch structure.
[0031] Secondly, the chain extenders used in the present invention are all diepoxy groups, which are different from commonly used chain extenders (such as pentaerythritol triacrylate and methyl propane triacrylate). Under the synergistic effect of peroxide initiators and process adjustments, the epoxy groups are more inclined to react with the terminal carboxyl groups of PLA. In addition, the reactivity of the epoxy groups is relatively low, and side reactions such as self-polymerization will not occur during the reaction process, which effectively improves the melt strength and expansion ratio of PLA while reducing costs. The selected bifunctional structure reduces the reaction sites compared to the multifunctional structure, is more conducive to reducing the cross-linked structure, and greatly retains the degradability of the PLA material.
[0032] Thirdly, the present invention optimizes the ratio of oxide initiator and chain extender, so that the PLA foaming material can obtain a higher melt strength improvement at a lower degree of crosslinking, can effectively support the expansion of bubbles, and does not collapse at a higher foaming ratio.
[0033] Finally, the present invention optimizes the screw structure of the extruder, sets a group of reverse conveying elements, prolongs the residence time of the material in the barrel, makes the PLA, chain extender and peroxide initiator mixed evenly, reacts more fully, and improves the long branching rate of PLA. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the SEM image of the PLA foam material in Example 1;
[0035] Figure 2 This is the SEM image of the PLA foam material of Example 3;
[0036] Figure 3 This is the SEM image of PLA foam material in Comparative Example 1;
[0037] Figure 4 This is the SEM image of PLA foam material of Comparative Example 2;
[0038] Figure 5 A schematic structural diagram of an improved twin-screw extruder in the embodiment;
[0039] Figure 6 for Figure 5 Schematic diagram of the forward conveying element of the middle screw;
[0040] Figure 7 for Figure 5 Schematic diagram of the mixing element of the middle screw;
[0041] Figure 8 for Figure 5 Schematic diagram of the reverse conveying element of the middle screw;
[0042] The reference numerals are: 1 hopper, 2 screw, 2-1 forward conveying element, 2-2 mixing element, 2-3 reverse conveying element, 3 liquid feed. DETAILED DESCRIPTION
[0043] The above scheme is further described below in conjunction with specific embodiments. The following factual cases are only used for the method used in the present invention, and the specific implementation conditions can be adjusted according to the manufacturer's needs and conditions.
[0044] The specific brands of raw materials used in the following embodiments and comparative examples of the present invention are: PLA (brand LX175), peroxide initiator 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (brand Trigonox 301), di-tert-butyl peroxide (brand Trigonox B), tert-amyl peroxide pivalate (brand ZH-TAPP), diisopropyl peroxydicarbonate (brand SSBT).
[0045] Example 1
[0046] A supercritical foamed PLA material, comprising the following mass fractions:
[0047] PLA 99.25%, peroxide initiator 0.25%, chain extender 0.5%; wherein the peroxide initiator is 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, and the chain extender is 1,6-hexanediol diglycidyl ether.
[0048] A method for preparing a supercritical foamed PLA material based on the above includes the following steps:
[0049] Step (1) weigh PLA, peroxide initiator and chain extender according to mass fraction.
[0050] Step (2) The components weighed in step (1) are placed in a low-speed mixer and blended for 20 minutes to obtain a mixed material.
[0051] Step (3) vacuum-drying the mixture obtained in step (2) and then adding it to a twin-screw extruder; the twin-screw extruder is divided into five parts: forward conveying, mixing, reverse conveying, secondary forward conveying, and die, and the temperature of each part is set as follows: forward conveying is 140°C to 180°C, the mixing element is 180°C, the reverse conveying is 180°C, and the temperature is gradually increased from 180°C to 190°C at the secondary forward conveying to the die; the extruder has a screw aspect ratio of 64:1 or more, a screw speed of 50rpm to 400rpm, and extrusion granulation is performed to obtain LCB-PLA particles.
[0052] Step (4) The LCB-PLA particles obtained in step (3) are vacuum dried at 70° C. for 2 h and then pressed into sheets using a flat vulcanizer at 180° C.
[0053] Step (5) Place the sheet obtained in step (4) into a supercritical CO2 foaming reactor, heat it to 125°C, use a constant pressure injection pump to inject CO2 into the reactor until the pressure in the reactor is 15MPa, saturate for 2h, release the pressure in the reactor to normal pressure within 2s, cool it to room temperature, and discharge the material to obtain PLA foaming material.
[0054] Example 2
[0055] The dosage of initiator and chain extender was adjusted, and the mass fraction of raw materials was: PLA 95.75%, peroxide initiator 0.25%, chain extender 4%. The other steps were the same as in Example 1.
[0056] Example 3
[0057] The amount of chain extender was adjusted, and the mass fraction of raw materials was: PLA 95.25%, peroxide initiator 0.75%, chain extender 4%, and other steps were the same as in Example 1.
[0058] Example 4
[0059] Diglycidyl ether was selected as the chain extender, and the mass fraction of the raw materials was: PLA 97.75%, peroxide initiator 0.75%, and chain extender 1.5%. The other steps were the same as in Example 1.
[0060] Example 5
[0061] Bisphenol A diglycidyl ether was selected as the chain extender, and the mass fraction of the raw materials was: PLA 97.75%, peroxide initiator 0.75%, and chain extender 1.5%. The other steps were the same as in Example 1.
[0062] Example 6
[0063] Bisphenol A diglycidyl ether was selected as the chain extender, and the mass fraction of the raw materials was: PLA 96.25%, peroxide initiator 0.75%, and chain extender 3%. The other steps were the same as those in Example 1.
[0064] Example 7
[0065] Di-tert-butyl peroxide was used as a peroxide initiator. The mass fraction of the raw materials was: PLA 98.25%, peroxide initiator 0.75%, chain extender 1%. The other steps were the same as those in Example 1.
[0066] Comparative Example 1
[0067] The preparation method of the PLA foam material in Example 1 is used without using a chain extender or a peroxide initiator, and the mass fraction of the raw material is: PLA 100%.
[0068] Comparative Example 2
[0069] According to the preparation method of the PLA foam material in Example 1, no chain extender is used, and the mass fraction of the raw materials is: PLA 99.9%, peroxide initiator 0.1%.
[0070] Comparative Example 3
[0071] According to the preparation method of the PLA foam material in Example 1, no chain extender is used, and the mass fraction of the raw materials is: PLA 99.5%, peroxide initiator 0.5%.
[0072] Comparative Example 4
[0073] According to the preparation method of the PLA foam material in Example 1, no chain extender is used, and the mass fraction of the raw materials is: PLA 99.25%, peroxide initiator 0.75%.
[0074] Comparative Example 5
[0075] According to the preparation method of the PLA foam material in Example 1, no chain extender is used, and the mass fraction of the raw materials is: PLA 98.75%, peroxide initiator 1.25%.
[0076] Comparative Example 6
[0077] According to the preparation method of the PLA foam material in Example 1, no chain extender is used, and the mass fraction of the raw materials is: PLA 98.5%, peroxide initiator 1.5%.
[0078] Comparative Example 7
[0079] According to the preparation method of the PLA foam material in Example 1, trimethylolpropane triacrylate (TMPTA) was used as a chain extender, and the mass fraction of the raw materials was: PLA 98.25%, peroxide initiator 0.75%, and chain extender 1%.
[0080] Comparative Example 8
[0081] According to the preparation method of the PLA foam material in Example 1, dicumyl peroxide (DCP) was used as a peroxide initiator, and the mass fractions of the raw materials were: PLA 98.25%, peroxide initiator 0.75%, and chain extender 1%.
[0082] Table 1: Foam density, expansion ratio and gel content of examples and comparative examples
[0083]
[0084]
[0085] As can be seen from Table 1, the foaming ratio of the PLA foam material prepared by the present invention is greater than 30, and a large improvement in melt strength is obtained at a lower degree of crosslinking, which can effectively support the expansion of bubbles and keep the pore shape from collapsing at a high foaming ratio ( Figure 1 , Figure 2 ). In addition, the crosslinking produced by the chain extender used in the present invention is very small, which is conducive to retaining the degradation performance of PLA. In Comparative Example 7, trimethylolpropane triacrylate is selected as the chain extender, which reacts with the hydroxyl and carboxyl groups in PLA, resulting in a higher degree of crosslinking of the modified PLA, affecting its foaming performance.
[0086] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A supercritical foamed PLA material, characterized in that: The components include the following mass fractions: PLA 95.25%~99.25%; Peroxide initiator 0.25% to 0.75%; Chain extender 0.5% to 4%; The peroxide initiator is one of 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, di-tert-butyl peroxide, tert-amyl peroxypivalate, and diisopropyl peroxydicarbonate, or a mixture of any two or more thereof in any ratio.
2. A supercritical foamed PLA material according to claim 1, characterized in that: The chain extender is any one of 1,6-hexanediol diglycidyl ether, 1,3-diepoxyglyceryl ether glycerol, diglycidyl ether, 1,4-bis(oxyglycidyl)benzene, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, and bisphenol A diglycidyl ether, or a mixture of any two or more of them in any ratio.
3. A method for preparing a supercritical foamed PLA material, comprising the following steps: Step (1): weighing PLA, peroxide initiator, and chain extender according to mass fraction; Step (2): placing the components weighed in step (1) in a blender and mixing them evenly; Step (3): drying the mixture obtained in step (2) and adding it to a twin-screw extruder for extrusion and granulation to obtain LCB-PLA particles; Step (4): drying the LCB-PLA particles obtained in step (3) and then subjecting the particles to a flat vulcanizing machine to obtain a sheet; Step (5): placing the sheet obtained in step (4) into a supercritical foaming reactor, heating it to the foaming temperature, introducing a supercritical fluid into the reactor, foaming, and rapidly releasing the pressure to obtain a PLA foaming material.
4. The method for preparing supercritical foamed PLA material according to claim 3, characterized in that: In step (2), the mixing time of the raw materials in the mixer is 20 min to 30 min; and the drying temperature of the mixed material in step (3) is 60° C. to 80° C., and the drying time is 2 h to 6 h.
5. The method for preparing supercritical foamed PLA material according to claim 3, characterized in that: In the step (3), the twin-screw extruder is divided into five parts: forward conveying, mixing, reverse conveying, secondary forward conveying, and a die; the screw length-to-diameter ratio of the twin-screw extruder is greater than 64:1, and the rotation speed is 50 rpm to 400 rpm; the temperature of the twin-screw extruder is 140° C. to 190° C.
6. The method for preparing supercritical foamed PLA material according to claim 3, characterized in that: In the step (4), the drying treatment temperature is 60°C to 80°C, and the drying time is 2h to 6h; and the temperature of the flat vulcanizing press in the step (4) is 180°C.
7. The method for preparing supercritical foamed PLA material according to claim 3, characterized in that: The supercritical fluid in step (5) is supercritical CO2.
8. A supercritical foamed PLA material according to claim 3, characterized in that: In the step (5), the foaming temperature is 115° C. to 135° C.; the foaming fluid pressure is 5 MPa to 15 MPa, and the time is 0.5 h to 2 h.
9. A supercritical foamed PLA material according to claim 3, characterized in that: The pressure relief time in step (5) is 2 seconds, and the kettle can be opened to discharge the material after the pressure is reduced to normal pressure.
Citation Information
Cited By
Multilayer composite material, preparation method and application thereof
CN121588264A
A multilayer composite, a method of manufacture and use thereof
CN121588264B