UV (ultraviolet) visbreaking point and point adhesive as well as preparation method and application of UV visbreaking point and point adhesive

By using acrylate oligomers and free radical photoinitiators, combined with vapor phase silica and curing retardant, the problem of UV detoxification dot dispensing cannot quickly lose sticking under low light, and the use in daily life is achieved fast detachment effect and high cohesion strength.

CN119060657APending Publication Date: 2024-12-03DELI GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187794.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing UV sticky spot glue cannot lose its stickiness quickly under low light intensity and cannot meet the needs of daily life.

Method used

Acrylate oligomers are used as the main body, and a radical photoinitiator and vapor-phase silica are combined to form a UV adhesive reducing adhesive composition. The reaction speed and cohesion intensity are adjusted by curing retardant agent to ensure rapid under low light intensity Loss of stickiness.

Benefits of technology

It realizes the effect of rapid detachment at low light intensity (about 3mw/cm2), and at the same time improves the cohesive strength and anti-static properties of the colloid, reduces residual glue phenomenon and wire drawing problems, and ensures pattern integrity and production aging. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060657A_ABST
    Figure CN119060657A_ABST
Patent Text Reader

Abstract

The invention relates to a UV (ultraviolet) visbreaking point-point adhesive as well as a preparation method and application of the UV visbreaking point-point adhesive, the UV visbreaking point-point adhesive comprises a UV visbreaking adhesive composition, and the UV visbreaking adhesive composition comprises the following raw materials in parts by weight: 100 parts of acrylic resin, 0.1-3 parts of a curing agent, 0.5-5 parts of a curing retarder, 0.1-3 parts of a UV initiator and 0.5-5 parts of fumed silica. According to the invention, the acrylate oligomer is used as a main body, has more functional groups and active groups, and can be matched with the UV initiator to rapidly react under low illumination intensity, and meanwhile, the UV initiator is a free radical type photoinitiator, and the initiator has the characteristics of high photosensitivity, high reaction speed, high light energy utilization rate and the like; when being matched with acrylate oligomer glue with multiple functional groups and multiple active groups, the adhesive can quickly lose viscosity under low illumination intensity (about 3mw / cm < 2 >).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of UV viscosity-reducing adhesive compositions, and in particular to a UV viscosity-reducing point-dispensing adhesive and a preparation method thereof. Background Art

[0002] Dot glue is a common stationery product. It is an adhesive that usually appears in the form of tape, glue stick, glue dots, etc. Dot glue has the following advantages:

[0003] (1) Dot glue is very convenient to use. It can be used to bond various materials, including paper, cardboard, cloth, plastic, etc. Whether it is repairing books, making handicrafts or organizing research notes, dot glue is an essential tool. Especially when repairing paper, the use of dot glue can avoid excessive glue flow and ensure the neatness of the repair process;

[0004] (2) Dot glue has a high viscosity, can provide a strong bond, and can maintain long-term durability. Compared with other disposable glues, dot glue is more durable and not easy to fall off or fail, which makes it an ideal choice for bonding important documents, promotional materials, posters, etc.

[0005] (3) Dot glue is a safe, non-toxic adhesive suitable for children. Children can use it to carry out handicrafts, collages, paper cutting and other activities, which not only exercises their hands-on ability but also improves their creativity and imagination.

[0006] When using dot glue to stick documents, notes, and decorations in daily life, it is common to make mistakes when sticking or to remove them after a period of time, which will damage the paper or other adhered objects. If you choose a low-viscosity dot glue, the sticking strength will not be enough. Therefore, it is extremely important to choose a dot glue that has good viscosity but can lose viscosity under certain conditions.

[0007] There are many point-dispensing adhesives with specific properties disclosed in the prior art, such as:

[0008] CN 114517069 A discloses a UV anti-viscosity adhesive tape, wherein the adhesive composition provided comprises 100.0 parts by weight of (methyl) acrylate copolymer, 1.0-10.0 parts by weight of aromatic polyurethane acrylate oligomer containing 6 vinyl groups, 0.5-5.0 parts by weight of curing agent, and 3.0 parts by weight of photoinitiator. After curing, the adhesive composition forms a UV anti-viscosity adhesive layer, and the UV anti-viscosity adhesive layer has low peeling force after high temperature treatment and UV treatment. CN 113755110 A discloses a UV anti-viscosity adhesive film, comprising a primer layer, a substrate layer, an anti-viscosity adhesive layer and a release film layer which are sequentially stacked; the anti-viscosity adhesive layer is made of a UV anti-viscosity adhesive composition; the UV anti-viscosity adhesive composition comprises the following components in parts by weight: 100 parts of acrylic resin, 0.9-2.8 parts of curing agent, 2-5 parts of antistatic agent and 0.9-2.5 parts of initiator, and the UV anti-viscosity adhesive film has lower haze, higher transparency and better antistatic property. CN 115197662 A discloses a UV viscosity-reducing adhesive and a UV viscosity-reducing film. The UV viscosity-reducing adhesive comprises, by weight, 100 parts of acrylic resin, 0.5-2 parts of curing agent, 0.3-3 parts of photoinitiator, 7-10 parts of cellulose ester, 0.1-3 parts of polyethylene glycol derivative, and 30-50 parts of solvent; the UV viscosity-reducing film comprises a substrate layer, a UV viscosity-reducing adhesive layer and a release film which are sequentially stacked, the UV viscosity-reducing adhesive layer is formed by thermally curing the UV viscosity-reducing adhesive, and the UV viscosity-reducing adhesive and UV viscosity-reducing film products have good storage stability, a long shelf life, and can meet use requirements. CN 114644900 A discloses a UV viscosity-reducing composition and a UV viscosity-reducing tape. The UV viscosity-reducing composition comprises: 50-100 parts by weight of a carboxyl-containing acrylate pressure-sensitive adhesive, 2-50 parts by weight of a multifunctional acrylate compound, 1-20 parts by weight of an auxiliary agent, 0.001-0.5 parts by weight of a curing agent, 0.001-0.5 parts by weight of a curing accelerator, and 0.1-3 parts by weight of a photoinitiator; wherein the auxiliary agent contains an active group, and the active group includes at least one of an epoxy group and an amino group. During the aging process of the composition, double bonds can be grafted onto the side chains of the pressure-sensitive adhesive, thereby achieving the advantages of increasing the molecular weight and reducing residual adhesive.

[0009] In the existing technology, the viscosity and no residual adhesive performance of UV detackifying adhesives have been greatly improved, but there has been no significant progress in rapid detackification. At present, UV detackifying adhesives are all used in the electronics industry or industrial processes, and there is no precedent for their application in dispensing glue. The intensity of UV light used in industry is high, about 200mw / cm 2 , which can quickly provide a large amount of energy to the UV adhesive. However, dispensing glue is mostly used in daily life. The UV light source in daily life is generally sunlight, ultraviolet lamps or banknote detectors, etc. The light intensity is relatively low, about 3mw / cm 2Under such light intensity, UV detackifying glue cannot lose viscosity quickly and cannot meet the needs of daily life.

[0010] Therefore, further improvements are needed for the current UV viscosity-reducing point dispensing process. Summary of the invention

[0011] The first technical problem to be solved by the present invention is to provide a UV viscosity-reducing point dispensing glue which has high viscosity, no residual glue and can quickly lose viscosity under low light intensity in view of the current status of the prior art.

[0012] The second technical problem to be solved by the present invention is to provide a preparation method of UV viscosity-reducing point dispensing glue in view of the current status of the prior art.

[0013] The third technical problem to be solved by the present invention is to provide an application of UV viscosity-reducing point dispensing glue in daily life in view of the current status of the prior art.

[0014] The technical solution adopted by the present invention to solve at least one of the above technical problems is:

[0015] A UV anti-viscosity point dispensing glue, comprising a UV anti-viscosity adhesive composition, wherein the raw materials used in the UV anti-viscosity adhesive composition include 100 parts of acrylic resin, 0.1-3 parts of curing agent, 0.5-5 parts of curing retarder, 0.1-3 parts of UV initiator and 0.5-5 parts of fumed silica according to weight components;

[0016] The acrylic resin is an acrylic acid ester oligomer formed by initiation polymerization;

[0017] The UV initiator is a free radical photoinitiator;

[0018] After production is completed, the curing retarder is eliminated by volatilization.

[0019] Preferably, the acrylic resin is an acrylic acid ester oligomer prepared by initiating polymerization with one or more of ammonium persulfate, benzoyl peroxide, and diisopropyl peroxide, and has a weight average molecular weight of 500,000-1,000,000.

[0020] Preferably, the solid content of the acrylic resin is 40-60%; the viscosity of the acrylic resin is 1000-10000 mPa.s; and the glass transition temperature of the acrylic resin is -60 to -20°C.

[0021] Preferably, the fumed silica is hydrophobic silica prepared by a gas phase method and post-treated with silane, and the fumed silica is used to provide physical crosslinking points that can cooperate with the curing agent to crosslink during the production process and fail in a high-temperature use environment.

[0022] Preferably, the acrylic resin is one or more of 2-ethylhexyl acrylate, hydroxyethyl acrylate, acrylic acid, isobornyl acrylate, isobornyl methacrylate, methyl methacrylate, isodecyl acrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl methacrylate, acryloylmorpholine, acrylamide, methacrylamide, 4-hydroxybutyl acrylate, and styrene.

[0023] Preferably, the UV initiator is one or more of 1-hydroxycyclohexyl benzophenone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 4-methylbenzophenone, methyl benzoylformate, and benzoin diethyl ether. Its function is that the excited state generated after light irradiation is to induce a pair of free radicals by homolytic cleavage of intramolecular chemical bonds or to generate free radicals by bimolecular hydrogen abstraction reaction between the excited state and the substrate, and one or both free radicals can further initiate the photopolymerization of the monomer.

[0024] The fumed silica of the present invention is a hydrophobic fumed silica obtained by post-treatment with silane. Its function is to improve the cohesion, heat resistance and antistatic properties of the colloid by adding silica as a physical crosslinking point in the colloid, and the addition of silica helps to adjust the fluidity of the glue and improve the coating properties of the production.

[0025] Preferably, the curing agent is one or more of hexamethylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, toluene diisocyanate, polymethylene phenyl polyisocyanate, 1,1,1-trimethylolpropane, and toluene diisocyanate adducts; the curing retarder is methyl ethyl ketone. The curing agent can react with the active functional groups contained in the polymer to form a three-dimensional network structure, improve product stability, and optimize product performance; the curing retarder can delay the reaction between the curing agent and the acrylic resin through the difference in solubility, thereby achieving the purpose of reducing pre-crosslinking and improving performance stability, and can greatly improve the timeliness of glue production.

[0026] Preferably, the UV viscosity-reducing point-dispensing glue of the present invention comprises a low release force layer, a substrate layer, a high release force layer and a point-dispensing glue layer which are sequentially stacked;

[0027] The thickness of the high release force layer and the low release force layer are both 0.1-2μm; the thickness of the substrate layer is 10-30μm; the thickness of the UV viscosity reducing point dispensing layer is 10-50μm;

[0028] The dot-adhesive layer is made of the UV viscosity-reducing adhesive composition; the high release force layer and the low release force layer are both made of organic silicone oil, and the organic silicone oil is selected from one or more of ethyl silicone oil, phenyl silicone oil, methyl hydrogen silicone oil, methyl phenyl silicone oil, methyl chlorophenyl silicone oil, methyl ethoxy silicone oil, methyl trifluoropropyl silicone oil, methyl vinyl silicone oil, methyl hydroxy silicone oil, ethyl hydrogen silicone oil, hydroxy hydrogen silicone oil, and cyanide silicone oil; the substrate layer is made of polyethylene terephthalate.

[0029] The raw materials of the UV viscosity-reducing adhesive composition of the present invention further include one or more solvents selected from the group consisting of ethyl acetate, methyl acetate, toluene, xylene, hexane, cyclohexane, acetone, and acetylacetone.

[0030] A method for preparing the above-mentioned UV viscosity-reducing point dispensing glue comprises the following steps:

[0031] (1) uniformly mixing an acrylic resin, a curing agent, a curing retarder, a UV initiator, fumed silica and a solvent to obtain a UV viscosity-reducing adhesive composition, wherein the solid content of the UV viscosity-reducing adhesive composition is 20-40%;

[0032] (2) placing the uniformly mixed UV viscosity-reducing adhesive composition in a degassing machine for degassing; degassing conditions: setting the air pressure to 0.01 MPa and the time to 5-15 min;

[0033] (3) applying the degassing UV adhesive to the high release force layer of the release film, and then drying it in an oven; drying conditions: temperature 80-120° C., drying time 1-5 min;

[0034] (4) After drying, the adhesive is further placed in a curing oven for curing under the following curing conditions: temperature 30-60° C., curing time 1-4 days; and the UV viscosity-reducing point dispensing adhesive is obtained.

[0035] An application of the above-mentioned UV viscosity-reducing point glue, wherein the UV viscosity-reducing point glue is used for light intensity of 2 to 5 mw / cm 2 Under the light source. Especially about 3mw / cm 2 Under light sources, such as UV light sources such as sunlight, ultraviolet lamps or banknote detectors in daily life.

[0036] Compared with the prior art, the advantages of the present invention are as follows: the present invention adopts acrylate oligomer as the main body, which has more functional groups and active groups, and can react quickly under low light intensity with UV initiator. At the same time, the UV initiator in the present invention selects free radical photoinitiator, which has the characteristics of strong photosensitivity, fast reaction speed, high light energy utilization rate, etc., and can be matched with acrylate oligomer glue with multiple functional groups and multiple active groups to react quickly under low light intensity (about 3mw / cm2 ) Rapid loss of adhesion;

[0037] Since the polymerization degree of acrylic acid oligomers is low, if the cohesive strength of the product is insufficient during direct production, it is easy to cause residual glue, poor aging performance and other problems. In order to solve this problem, the present invention also adds a curing agent and hydrophobic silica prepared by the gas phase method. The curing agent can pre-crosslink the acrylic glue to provide sufficient cohesive strength for the colloid, and the hydrophobic silica prepared by the gas phase method can cooperate with the curing agent as a physical crosslinking point in the colloid to further enhance the cohesive strength of the colloid. In addition, although the gas phase silica as a physical crosslinking point may affect the initial adhesion and peeling strength of the colloid to a small extent, the crosslinking point will fail at high temperature, thereby eliminating the effect on the initial adhesion and peeling strength of the colloid; at the same time, the addition of gas phase silica can also solve the following two problems: (1) gas phase silica can effectively reduce the elongation at break of the colloid, thereby eliminating the problem of wire drawing that often occurs during the use of point glue; (2) gas phase silica can effectively inhibit the fluidity of the glue, which is beneficial to ensure the integrity of the pattern when coating and engraving various patterns during the production process of point glue;

[0038] The reaction between the acrylic glue with multiple functional groups and multiple active groups and the curing agent is relatively fast, which can easily lead to a decrease in the timeliness of the glue during the production process, and the performance difference of the product before and after the production is large. In order to solve this problem, the present invention adds a curing retarder to the formula system to avoid or slow down the premature reaction between the curing agent and the glue during the production process. As the production proceeds, the curing retarder completely evaporates and does not affect the performance of the product itself.

[0039] In the present application, the acrylic resin adopts acrylic acid ester oligomers, which is beneficial to enhance the cohesive strength of the colloid and is not prone to residual glue. In addition, by adding fumed silica to act as the physical cross-linking point inside the colloid, it is beneficial to further reduce the residual glue phenomenon. By adding a curing retarder, the purpose of slowing down the pre-cross-linking is achieved, thereby ensuring the stability of product performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic structural diagram of an embodiment of the present invention. DETAILED DESCRIPTION

[0041] The present invention is further described in detail below with reference to the accompanying drawings.

[0042] like Figure 1 As shown, the UV viscosity-reducing point-dispensing glue of the embodiment of the present invention comprises a low release force layer 4, a substrate layer 3, a high release force layer 2 and a point-dispensing glue layer 1 which are stacked in sequence.

[0043] The thickness of the high release force layer 2 and the low release force layer 4 are both 0.5 μm; the thickness of the substrate layer 3 is 12 μm; and the thickness of the dot-adhesive layer 1 is 25 μm.

[0044] The dot glue layer 1 is made of a UV-tackifying adhesive composition; the high release layer 2 and the low release layer 4 are both made of silicone oil; and the substrate layer 3 is made of polyethylene terephthalate. The high release layer 2, the low release layer 4, and the substrate layer 3 of this embodiment are all purchased directly from Wenzhou Xinfeng Composite Materials Co., Ltd.

[0045] The preparation method of the UV viscosity reducing point dispensing glue of the embodiment of the present invention is:

[0046] The uniformly mixed UV viscosity-reducing adhesive composition is placed in a degassing machine for degassing treatment, and the air pressure is set to 0.01 MPa for 10 minutes. The release film is placed flat on the coating machine table with the high release force side facing upward, and the vacuum pump is turned on to adsorb the release film on the coating machine table. The UV viscosity-reducing adhesive composition after the degassing treatment is coated using the YOSHIMITSU SEIKI precision coater YBA-5 of Kodaira Manufacturing Co., Ltd., Japan, and the wet adhesive thickness is 100 μm. The coated sample is placed in a blast oven for drying at a temperature of 90°C and a drying time of 2 minutes. A new release film is taken, and the dried sample adhesive surface and the low release surface are laminated with a laminating machine, and the laminating machine pressure is 100N. The above-prepared sample is placed in an aging oven for aging treatment, and the aging temperature is 30-60°C and the aging time is 1-4 days.

[0047] Embodiment 1:

[0048] The UV viscosity reducing adhesive composition in this embodiment includes the following components in parts by weight:

[0049]

[0050] Among them, the acrylic resin is KP977S from Yashiya, the curing agent is CK401E from Yashiya, the curing retarder is methyl ethyl ketone, the UV initiator is BASF's 184, and the fumed silica is HT901 from Huating Nano.

[0051] The preparation method of the UV anti-tack adhesive composition is:

[0052] Add acrylic resin, curing retarder and solvent (ethyl acetate) into a measuring cup, and stir them uniformly with a glass rod for 2 minutes to make them evenly mixed; then add fumed silica into the stirred glue, and stir them uniformly with a glass rod for 3 minutes; add curing agent into the stirred glue, and stir them uniformly with a glass rod for 3 minutes; finally, add UV initiator into the stirred glue, and place it in a centrifugal disperser. The centrifuge parameters are set as follows: stage one speed 1000r / min time 25min, stage two speed 2000r / min time 5min, and the desired UV viscosity-reducing adhesive composition is obtained after centrifugal dispersion, and its solid content is between 20-40%.

[0053] Embodiment 2:

[0054] The UV viscosity-reducing adhesive composition of this embodiment includes the following components in parts by weight:

[0055]

[0056] Among them, the acrylic resin is KP977S from Yashiya, the curing agent is CK401E from Yashiya, the curing retarder is methyl ethyl ketone, the UV initiator is BASF's 184, and the fumed silica is HT901 from Huating Nano.

[0057] The preparation method of the UV anti-tack adhesive composition is consistent with that of Example 1.

[0058] Embodiment 3:

[0059] The UV viscosity-reducing adhesive composition of this embodiment includes the following components in parts by weight:

[0060]

[0061] Among them, the acrylic resin is KP977S from Yashiya, the curing agent is CK401E from Yashiya, the curing retarder is methyl ethyl ketone, the UV initiator is BASF's 184, and the fumed silica is HT901 from Huating Nano.

[0062] The preparation method of the UV anti-tack adhesive composition is consistent with that of Example 1.

[0063] Embodiment 4:

[0064] The UV viscosity-reducing adhesive composition of this embodiment includes the following components in parts by weight:

[0065]

[0066] Among them, the acrylic resin is KP977S from Yashiya, the curing agent is CK401E from Yashiya, the curing retarder is methyl ethyl ketone, the UV initiator is BASF's 184, and the fumed silica is HT901 from Huating Nano.

[0067] The preparation method of the UV anti-tack adhesive composition is consistent with that of Example 1.

[0068] Embodiment 5:

[0069] The UV viscosity-reducing adhesive composition of this embodiment includes the following components in parts by weight:

[0070]

[0071] Among them, the acrylic resin is KP977S from Yashiya, the curing agent is CK401E from Yashiya, the curing retarder is methyl ethyl ketone, the UV initiator is BASF's 184, and the fumed silica is HT901 from Huating Nano.

[0072] The preparation method of the UV anti-tack adhesive composition is consistent with that of Example 1.

[0073] Comparative Example 1:

[0074] The UV anti-tack adhesive composition of this comparative example includes the following components in parts by weight:

[0075]

[0076] The components and preparation methods are consistent with those in Example 1.

[0077] Comparative Example 2:

[0078] The UV anti-tack adhesive composition of this comparative example includes the following components in parts by weight:

[0079]

[0080] The components and preparation methods are consistent with those in Example 1.

[0081] Comparative Example 3:

[0082] The UV anti-tack adhesive composition of this comparative example includes the following components in parts by weight:

[0083]

[0084] The components and preparation methods are consistent with those in Example 1.

[0085] Comparative Example 4:

[0086] The UV anti-tack adhesive composition of this comparative example includes the following components in parts by weight:

[0087]

[0088] The components and preparation methods are consistent with those in Example 1.

[0089] Comparative Example 5:

[0090] The UV anti-tack adhesive composition of this comparative example includes the following components in parts by weight:

[0091]

[0092] Among them, the acrylic resin is specifically Yashiya PE123N (this glue is not an acrylate oligomer).

[0093] The components and preparation methods are consistent with those in Example 1.

[0094] In order to compare and illustrate the performance of the UV viscosity-reducing point-dispensing adhesives prepared in Examples 1-5 and Comparative Examples 1-5, the prepared UV viscosity-reducing point-dispensing adhesives were subjected to the following performance tests.

[0095] 1. Adhesive tape peel strength test:

[0096] The test method for the force required to remove an adhesive tape from stainless steel at 180° is specified. An adhesive tape is attached to a stainless steel plate, which is fixed to a fixture of a tensile testing machine. The other fixture of the testing machine clamps the free end of the adhesive tape at 180° to the stainless steel plate, and the adhesive tape is pulled apart at a specified rate. The peel force is measured by the force required to continuously peel the adhesive tape from the stainless steel plate and converted into peel strength. Note that the peel line is perpendicular to the direction of the force. For specific test methods, refer to GB / T 2792-2014.

[0097] 2. Release film 180° peeling force test:

[0098] The load required to continuously peel a test strip of a certain width at a certain speed under the peeling condition of a peeling angle of 180°. It is expressed in mN / 25mm. For specific test methods, refer to GB / T 25256-2010.

[0099] 3. Initial adhesion test of pressure-sensitive adhesive tape:

[0100] Roll a steel ball over the sticky surface of the adhesive tape placed flat on an inclined plate, and evaluate its initial tack based on the maximum steel ball size that can be adhered to the sticky surface of a specified length; or roll a steel ball of a specified size over an inclined groove, and measure the distance it rolls on the sticky surface of the adhesive tape on a horizontal plate to evaluate its initial tack. For specific test methods, refer to GB / T4852-2002.

[0101] 4. Test of adhesive tape's stickiness:

[0102] The adhesion of the adhesive tape to the standard steel plate is measured by the failure time of the adhesive tape under constant load, temperature of (23±1)℃ and relative humidity of (50±5)%. A piece of adhesive tape is attached to a standard steel plate at a controlled rolling rate. The steel plate is installed vertically, and a standard mass weight is hung at the free end of the adhesive tape to determine the adhesion failure time. For specific test methods, refer to GB / T 4851-2014.

[0103] Since the test requires a substrate, the prepared UV anti-viscosity adhesive was applied to 25μm PET. Specifically, the low release film layer on the UV anti-viscosity adhesive was removed, the UV anti-viscosity adhesive layer was exposed, and the UV anti-viscosity adhesive layer was attached to the 25μm PET, and then pressed using a press to obtain a test sheet.

[0104] The UV light test method is: stick a 25mm wide test sheet on a standard test steel plate, cover it with an A4 white paper, and then expose it to UV light. Specifically, the UV light wavelength is 365nm and the light intensity is 3mw / cm 2 , the irradiation time is 2min.

[0105] Table 1 is the performance test results of Examples 1-5 and Comparative Examples 1-5:

[0106] Table 1

[0107]

[0108] As can be seen from Table 1, the comprehensive performance can be maintained good when the amount of curing agent added is controlled within the range defined by the present invention. A small amount of curing agent added will result in a small cohesive strength of the colloid, which will lead to a decrease in the holding viscosity; a large amount of curing agent added will result in a large cohesive strength, which will lead to a large release force and a small initial adhesion, and excessive cross-linking will lead to a poor UV viscosity reduction effect. The UV initiator also needs to be controlled within a certain range to ensure that the UV viscosity reduction effect maintains good comprehensive performance. Excessive addition of UV initiator leads to a decrease in holding viscosity and pre-UV peel strength, but at the same time, the post-UV peel strength will also be lower, and the viscosity reduction effect will be better. In the experiment, the more fumed silica is added, the greater the cohesive strength, the better the holding viscosity, and the less effect on other properties; it can be seen from Comparative Example 5 that the reaction of acrylate oligomers and UV initiators is more sufficient, and the viscosity reduction effect is better.

Claims

1. A UV viscosity-reducing point dispensing glue, comprising a UV viscosity-reducing adhesive composition, Features: According to the weight components, the raw materials used in the UV viscosity-reducing adhesive composition include 100 parts of acrylic resin, 0.1-3 parts of curing agent, 0.5-5 parts of curing retarder, 0.1-3 parts of UV initiator and 0.5-5 parts of fumed silica; The acrylic resin is an acrylic acid ester oligomer formed by initiation polymerization; The UV initiator is a free radical photoinitiator; After production is completed, the curing retarder is eliminated by volatilization.

2. The UV viscosity reducing point dispensing glue according to claim 1, Features: The acrylic resin is an acrylic acid ester oligomer prepared by initiating polymerization with one or more of ammonium persulfate, benzoyl peroxide and diisopropyl peroxide, and has a weight average molecular weight of 500,000 to 1,000,000.

3. The UV viscosity reducing point dispensing glue according to claim 2, Features: The solid content of the acrylic resin is 40-60%; the viscosity of the acrylic resin is 1000-10000 mpa.s; and the glass transition temperature of the acrylic resin is -60 to -20°C.

4. The UV viscosity reducing point dispensing glue according to any one of claims 1 to 3, Features: The fumed silica is a hydrophobic silica prepared by a gas phase method and post-treatment with silane. The fumed silica is used to provide physical crosslinking points that can cooperate with a curing agent to crosslink during the production process and fail in a high-temperature use environment.

5. The UV viscosity reducing point dispensing glue according to any one of claims 1 to 3, Features: The acrylic resin is one or more of 2-ethylhexyl acrylate, hydroxyethyl acrylate, acrylic acid, isobornyl acrylate, isobornyl methacrylate, methyl methacrylate, isodecyl acrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl methacrylate, acryloylmorpholine, acrylamide, methacrylamide, 4-hydroxybutyl acrylate, and styrene.

6. The UV viscosity reducing point dispensing glue according to any one of claims 1 to 3, Features: The UV initiator is one or more of 1-hydroxycyclohexyl benzophenone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 4-methylbenzophenone, methyl benzoylformate, and benzoin diethyl ether.

7. The UV viscosity reducing point dispensing glue according to any one of claims 1 to 3, Features: The curing agent is one or more of hexamethylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, toluene diisocyanate, polymethylene phenyl polyisocyanate, 1,1,1-trimethylolpropane, and adducts of toluene diisocyanate; and the curing retarder is methyl ethyl ketone.

8. The UV viscosity reducing point dispensing glue according to any one of claims 1 to 3, Features: It includes a low release force layer, a substrate layer, a high release force layer and a dot glue layer which are stacked in sequence; The dot-adhesive layer is made of the UV viscosity-reducing adhesive composition; the high release force layer and the low release force layer are both made of organic silicone oil, and the organic silicone oil is selected from one or more of ethyl silicone oil, phenyl silicone oil, methyl hydrogen silicone oil, methyl phenyl silicone oil, methyl chlorophenyl silicone oil, methyl ethoxy silicone oil, methyl trifluoropropyl silicone oil, methyl vinyl silicone oil, methyl hydroxy silicone oil, ethyl hydrogen silicone oil, hydroxy hydrogen silicone oil, and cyanide silicone oil; the substrate layer is made of polyethylene terephthalate.

9. A method for preparing the UV viscosity-reducing point-dispensing glue according to any one of claims 1 to 8, Features The following steps are involved: (1) uniformly mixing an acrylic resin, a curing agent, a curing retarder, a UV initiator, fumed silica and a solvent to obtain a UV viscosity-reducing adhesive composition, wherein the solid content of the UV viscosity-reducing adhesive composition is 20-40%; (2) placing the uniformly mixed UV viscosity-reducing adhesive composition in a degassing machine for degassing; degassing conditions: setting the air pressure to 0.01 MPa and the time to 5-15 min; (3) applying the degassing UV adhesive to the high release force layer of the release film, and then drying it in an oven; drying conditions: temperature 80-120° C., drying time 1-5 min; (4) After drying, the adhesive is further placed in a curing oven for curing under the following curing conditions: temperature 30-60° C., curing time 1-4 days; and the UV viscosity-reducing point dispensing adhesive is obtained.

10. An application of the UV viscosity reducing point dispensing glue according to any one of claims 1 to 8, Features: The UV detackifying point dispensing glue is used for light intensity of 2 to 5 mw / cm 2 Under the light source.