Broadband-emission spectrum-adjustable yellow fluorescent powder and preparation method thereof

By introducing ethyl triphenylphosphine to non-lead perovskite phosphor to replace the Cs+ position, regulating the lattice field intensity of Sb3+, ETP2In1-xSbxCl5 phosphor was prepared, and the problems of Sb3+ ion excitation wavelength mismatch and high-temperature synthesis were solved. , achieving efficient photoluminescence and green industrial mass production.

CN119060725APending Publication Date: 2024-12-03NANKAI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411303996.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the optical properties of Sb3+ ions depend on the crystal field intensity of the matrix, resulting in a narrow excitation peak and does not meet the band of commercial ultraviolet chips, resulting in low light utilization, and high-temperature synthesis consumption and long time, making it difficult to achieve. Industrial mass production.

Method used

By introducing ethyl triphenylphosphine (ETP) to replace the Cs+ position in non-lead perovskite phosphor, the lattice field intensity of Sb3+ was regulated, and ETP2In1-xSbxCl5 phosphor was prepared, and the thermally-free solvent-free ethanol was used to achieve Sb3+ The excitation wavelength is adjusted to 365nm and the emission spectrum is broadened to match commercial ultraviolet chips.

Benefits of technology

The excitation wavelength of Sb3+ ions is matched with commercial ultraviolet chips, which improves photoluminescence efficiency, reduces synthesis energy consumption and time, supports green industrial mass production, and improves the quantum yield to nearly 100%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060725A_ABST
    Figure CN119060725A_ABST
Patent Text Reader

Abstract

The invention relates to yellow fluorescent powder with broadband emission and adjustable spectrum and a preparation method thereof. The structural formula of the fluorescent powder is ETP2In (1-x) SbxCl5, wherein x is more than or equal to 0.05 and less than or equal to 0.99, and ETP is ethyl triphenylphosphine. In preparation, ethanol is used as a solvent, and a powder product can be rapidly synthesized without heating. Rare earth ion doping is avoided, the excitation wavelength is matched with the wave band of a commercial ultraviolet chip, and the emission spectrum is adjustable; the solvent is non-toxic and non-corrosive, an oxidizing or reducing atmosphere is not needed, only a small amount of ethanol needs to be used for synthesis at room temperature, the reaction time is greatly shortened from several hours to minute or even second magnitude except a high-temperature condition is not needed, and green industrial mass production is supported.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a yellow light phosphor with broadband emission and adjustable spectrum and a preparation method thereof. Background Art

[0002] The development of lighting technology has greatly improved people's learning, working and living environment, but it has also introduced energy consumption issues. According to reports, in 2018, lighting accounted for 20% of global electricity consumption. Although fluorescent lamps have been gradually replaced by new LEDs in recent years, lighting electricity consumption still accounts for about 13%. Therefore, the development of efficient lighting LEDs has become a social concern. Among them, phosphor materials, as the core of lighting LEDs, play an important role. Improving their photoluminescence efficiency and regulating the excitation wavelength to match the luminescence band of commercial UV chips are the core issues to improve the efficiency of power conversion and reduce power consumption.

[0003] Compared with oxide phosphors, halide perovskite phosphors have lower formation energy, which supports liquid phase synthesis at room temperature. This not only avoids excessive reliance on energy during the synthesis process (oxides require high-temperature solid-phase reactions at 1000-1600°C and insulation time of several hours), but also meets the needs of industrial green mass production. 2+ To solve the toxicity problem, the academic community has tried to replace Pb in the lattice with non-toxic (or low-toxic) metal ions. 2+ It has launched a series of lead-free perovskite derivative fluorescent materials to address the safety risks in potential applications.

[0004] In non-lead perovskite phosphors, Sb 3+ The ions show excellent photoluminescence properties, and their fluorescence quantum yield often reaches about 90%. 3+ The optical properties of ions are heavily dependent on the crystal field strength of the matrix. Due to the crystal field limitation of inorganic materials, their excitation peaks are narrow and often located at 280-340nm (such as Chem. Mater. 2020, 32, 12, 5327–5334; Light Sci. APPl., 2023, 12, 75, etc.), which is inconsistent with the current commercial UV chip (365nm) band, resulting in low light utilization and other problems. Therefore, it is difficult to combine with commercial chips, which greatly limits the Sb 3+ The application value of ions in the field of lighting.

[0005] The document Inorg.Chem.2021,60,17837-17845 reports ETP2SbCl5 phosphor, its crystal structure and basic luminescence properties; Patent CN 114736127 A reports an antimony pentachloride fluorescent compound, crystal, preparation method and application thereof, with the general molecular structure of M2(SbCl5)Y a , where M is an organic compound, Y is water or ethanol, a=0, 0.5 or 1, and one of the M organic compounds is ETP. Both schemes use high temperature synthesis, which consumes electrical energy and takes a long time to synthesize. Summary of the invention

[0006] The purpose of the present invention is to address the problems existing in the current technology such as high material formation energy, high temperature or high pressure synthesis safety hazards, excessive consumption of rare earth resources, difficulty in batch industrial preparation, Sb 3+ The ion excitation wavelength does not match the commercial chip, and the like, and a yellow light phosphor with broadband emission and adjustable spectrum and a preparation method thereof are provided. The specific chemical expression of the phosphor is ETP2In 1-x Sb x Cl5 (0.05≤x≤0.99), where ETP is ethyltriphenylphosphine; through the organic cation group (ethyltriphenylphosphine ion, referred to as ETP + ) replace Cs + position, reducing the lattice field strength and Sb 3+ The optimal excitation wavelength is adjusted to 365nm and the excitation spectrum is further broadened (such as 250-450nm), which effectively solves the problem of its difficulty in combining with commercial chips; ethanol is used as a solvent in the preparation, and the powder product can be quickly synthesized without heating. In the present invention, there is no rare earth ion doping, the excitation wavelength matches the band of commercial ultraviolet chips, and the emission spectrum is adjustable; the solvent is non-toxic and non-corrosive, and no oxidizing or reducing atmosphere is required. Only a small amount of ethanol is needed for synthesis at room temperature. In addition to not requiring high temperature conditions, the reaction time is also greatly reduced from several hours to minutes or even seconds, supporting green industrial mass production.

[0007] The technical solution of the present invention is:

[0008] A yellow light phosphor with broadband emission and adjustable spectrum, the structural formula of which is ETP2In 1-x Sb x Cl5;

[0009] Wherein, 0.05≤x≤0.99, and ETP is ethyltriphenylphosphine.

[0010] The yellow light fluorescent powder with broadband emission and adjustable spectrum emits yellow fluorescence under the irradiation of ultraviolet light.

[0011] The method for preparing the broadband emission and spectrum-adjustable yellow light phosphor comprises the following steps:

[0012] (1) According to the ratio of the above salts, 1-x Sb x According to the corresponding amount ratio of substances in Cl5 (0.05≤x≤0.99), the compound containing ETP, the compound containing In, and the compound containing Sb are added into the container and mixed;

[0013] Wherein, the ETP-containing compound is the chloride of ETP, namely, ETPCl; the In-containing compound is the chloride or hydrated chloride of In; the Sb-containing compound is the chloride of Sb;

[0014] (2) adding anhydrous ethanol to the container and stirring at 1000-10000 rpm for 30 seconds to 10 minutes;

[0015] Wherein, 1-10 mL of anhydrous ethanol was added for every 2 mmol of ETP compound;

[0016] (3) Centrifuge the product for 1-5 minutes;

[0017] (4) After centrifugation, the supernatant is poured out, and the final precipitate is dried at 40-80° C. for 2-5 hours to obtain a yellow phosphor with broadband emission and tunable spectrum.

[0018] The centrifugal speed in step (3) is 3000-5000 rpm.

[0019] The essential features of the present invention are:

[0020] In terms of luminescence performance, the present invention synthesizes ETP2In by In / Sb hybridization scheme. 1-x Sb x Cl5, Sb 3+ The In / Sb ratio is adjusted to control the Sb 3+ The lattice field strength and electroacoustic coupling strength of the ions can achieve emission spectrum regulation and high-efficiency photoluminescence, and in Sb 3+ When the content is 70%-90%, the quantum yield (PLQY) of the product reaches nearly 100%. + Replace Cs in commonly used Cs2InCl5:Sb + bit, reducing Sb 3+ The lattice field intensity is increased to achieve excitation spectrum broadening and peak red shift regulation. The above effects lay the foundation for its application in lighting, color temperature regulation and optical anti-counterfeiting.

[0021] In terms of preparation, in the traditional hydrothermal method, after pouring ethanol into the reactor, it is generally directly sealed and sent to an oven to be heated to 100-200°C to increase solubility and internal pressure to promote raw material dissolution. It is difficult to achieve stirring operation in this environment, so it takes a long time to complete the dissolution of the raw materials and the uniform dispersion of ions, and then the target crystal product is gradually precipitated by slowly cooling. Since the raw materials involved in the present invention show good solubility (ethanol solvent) at room temperature, the closed heating operation in the traditional scheme can be abandoned and carried out directly in a room temperature environment. For this reason, the present invention can achieve rapid stirring operation to accelerate dissolution, promote uniform mixing of ions, and provide reaction energy, so that a product with uniform physical phase can be quickly obtained. The reaction mechanism is described as follows:

[0022] In the present invention, the reaction after adding ethanol is a continuous process, which is macroscopically manifested as a rapid reaction from raw material powder to product powder; while microscopically, the dissolution process shown in the following formula 1-3 and the recrystallization process shown in formula 4 occur:

[0023] ETPCl=ETP + +Cl - (1)

[0024] InCl3=In 3+ +3Cl - (2)

[0025] SbCl3=Sb 3+ +3Cl - (3)

[0026] 2ETP + +(1-x)In 3+ +xSb 3+ +5Cl - =ETP2In 1-x Sb x Cl5↓ (4)

[0027] Since the formation energy of the product is low, the free ions can easily combine quickly to obtain the product according to the feed ratio, and the phosphor preparation can be completed within tens of seconds to several minutes when stirred quickly.

[0028] The beneficial effects of the present invention are:

[0029] (1) The present invention achieves the regulation and broadening of the Sb ion excitation wavelength, so that its excitation wavelength conforms to the commercial 365nm ultraviolet chip (such as the attached Figure 3 , 7 , as shown in 10), laying the foundation for combining it with commercial UV chips to achieve lighting applications.

[0030] (2) The present invention achieves the shape control of the emission spectrum by adjusting the In / Sb ratio (see attached Figure 2 , 6 ) and further improvement of PLQY (such as the attached Fig.11 ), which lays the foundation for lighting color temperature control or anti-counterfeiting.

[0031] (3) The present invention does not require dangerous synthesis conditions such as high temperature, high pressure, and hydrogen atmosphere. It only requires a small amount of ethanol to be synthesized at room temperature. In addition to not requiring high temperature conditions, the reaction time is also greatly reduced from several hours to minutes or even seconds, supporting green industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 ETP2In obtained in Example 1 0.95 Sb 0.05 XRD spectrum of Cl5;

[0033] Figure 2 ETP2In obtained in Example 1 0.95 Sb 0.05 Fluorescence emission spectrum of Cl5;

[0034] Figure 3 ETP2In obtained in Example 1 0.95 Sb 0.05 Fluorescence excitation spectrum of Cl5, monitoring wavelength is 660nm;

[0035] Figure 4 ETP2In obtained in Example 1 0.95 Sb 0.05 Fluorescence excitation spectrum of Cl5, monitoring wavelength is 510nm;

[0036] Figure 5 ETP2In obtained in Example 2 0.1 Sb 0.9 XRD spectrum of Cl5;

[0037] Figure 6 ETP2In obtained in Example 2 0.1 Sb 0.9 Fluorescence emission spectrum of Cl5;

[0038] Figure 7 ETP2In obtained in Example 2 0.1 Sb 0.9 Fluorescence excitation spectrum of Cl5;

[0039] Figure 8 ETP2In obtained in Example 3 0.01 Sb 0.99 XRD spectrum of Cl5;

[0040] Fig. 9ETP2In obtained in Example 3 0.01 Sb 0.99 Fluorescence emission spectrum of Cl5;

[0041] Fig.10 ETP2In obtained in Example 3 0.01 Sb 0.99 Fluorescence excitation spectrum of Cl5;

[0042] Fig.11 ETP2In obtained in Example 4 1-x Sb x The PLQY curve of Cl5 (x = 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99) varies with the x value; DETAILED DESCRIPTION

[0043] Example 1: ETP2In 0.95 Sb 0.05 Cl5 Sample

[0044] 2 mmol ETPCl (0.6536 g) powder, 0.95 mmol InCl 3 (0.1764 g) powder and 0.05 mmol SbCl 3 (0.0114 g) powder were weighed into a test tube, 1 mL of anhydrous ethanol was added and stirred at 5000 rpm for 5 min.

[0045] After the preparation is completed, the mixture is centrifuged at 5000rpm-1min, and then the supernatant is removed, and the final precipitate is placed in an oven and dried at 40°C for about 5 hours. After being taken out and crushed, a white sample in the final powder form can be obtained.

[0046] Test conditions: The crystal structure of the sample was tested using a Rigaku X-ray diffractometer, with a Cu target as the radiation source, a tube voltage of 40 kV, a tube current of 40 mA, a scanning step of 0.02°, a scanning speed of 15° / min, and a scanning range of 10°-60°. The emission and excitation spectra of the sample were obtained by testing with an FS-5 spectrometer.

[0047] Experimental results: Figure 1 Given is ETP2In 0.95 Sb 0.05 From the XRD spectrum of Cl5, it can be seen that a crystalline powder product has been obtained through this experimental scheme;

[0048] Figure 2 Given is ETP2In 0.95 Sb 0.05The fluorescence emission spectrum of Cl5 covers the range of about 400-850nm, showing two emission peaks at 510 and 660nm, corresponding to ETP + Organic molecular clusters and Sb 3+ Ion emission, the final light color displayed is yellow fluorescence;

[0049] Figure 3 Given is the ETP2In when monitoring 660nm emission 0.95 Sb 0.05 The fluorescence excitation spectrum of Cl5 covers a range of about 250-500nm, and exhibits the strongest excitation effect at 365nm, corresponding to Sb 3+ The excitation energy band of the ion. In addition, the excitation peak at 290nm is attributed to the band gap transition;

[0050] Figure 4 Given is the ETP2In when monitoring 510nm emission 0.95 Sb 0.05 The fluorescence excitation spectrum of Cl5 covers a range of about 270-370nm, and exhibits the strongest excitation effect at about 330nm, corresponding to ETP + The excitation energy band of organic molecular clusters. In addition, the excitation peak at 290nm is attributed to the band gap transition;

[0051] Example 2: ETP2In 0.1 Sb 0.9 Cl5 Sample

[0052] 2 mmol ETPCl (0.6536 g) powder, 0.1 mmol InCl 3 (0.0184 g) powder and 0.9 mmol SbCl 3 (0.2053 g) powder were weighed into a mortar, 10 mL of anhydrous ethanol was added and stirred at 1000 rpm for 10 min.

[0053] After the preparation is completed, the mixture is centrifuged at 3000 rpm for 5 min, the supernatant is poured out, and the final precipitate is placed in an oven and dried at 80° C. for about 2 hours to obtain a final powder sample.

[0054] Test conditions: the same as in Example 1.

[0055] Experimental results: Figure 5 Given is ETP2In 0.1 Sb 0.9 From the XRD spectrum of Cl5, it can be seen that a crystalline powder product has been obtained through this experimental scheme;

[0056] Figure 6 Given is ETP2In 0.1 Sb0.9 The fluorescence emission spectrum of Cl5 covers about 450-850nm, and shows the best emission intensity around 600nm. 3+ The bimodal case of Sb 3+ When the content increases, the double peak emission changes to a single peak emission, which is due to the organic molecular clusters to Sb 3+ The energy transfer is caused by the change of crystal field strength. 3+ The original emission peak at 660nm is blue-shifted to 600nm, showing yellow light emission characteristics. 3+ Regulated by concentration changes;

[0057] Figure 7 Given is ETP2In 0.1 Sb 0.9 The fluorescence excitation spectrum of Cl5 covers about 250-450nm, and the optimal excitation effect is shown at 290 and 368nm, which correspond to the band gap transition and Sb 3+ Excitation band transition;

[0058] Example 3: ETP2In 0.01 Sb 0.99 Cl5 Sample

[0059] 2 mmol ETPCl (0.6536 g) powder, 0.99 mmol SbCl3 (0.2258 g) and 0.01 mmol InCl3·4H2O (0.0029 g) powder were weighed into a test tube, 5 mL of anhydrous ethanol was added and stirred at 10000 rpm for 30 s.

[0060] After the preparation is completed, the mixture is centrifuged at 4000 rpm for 2 min, the supernatant is poured out, and the final precipitate is placed in an oven and dried at 60° C. for about 2 hours to obtain a final powder sample.

[0061] Test conditions: the same as in Example 1.

[0062] Experimental results: Figure 8 Given is ETP2In 0.01 Sb 0.99 From the XRD spectrum of Cl5, it can be seen that a crystalline powder product has been obtained through this experimental scheme;

[0063] Fig. 9 Given is ETP2In 0.01 Sb 0.99 The fluorescence emission spectrum of Cl5 covers about 450-850nm, and shows the optimal emission intensity at 600nm yellow light;

[0064] Fig.10 Given is ETP2In 0.01 Sb 0.99 The fluorescence excitation spectrum of Cl5 covers about 250-450nm, and the optimal excitation effect is shown at 290 and 368nm, which correspond to the band gap transition and Sb 3+ Excitation band transition;

[0065] Example 4: ETP2In 1-x Sb x Cl5 (x = 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99) samples

[0066] 2 mmol ETPCl (0.6536 g) powder, (1-x) mmol SbCl3 (0.2281*(1-x) g) and x mmol SbCl3 (0.2053*x g) powder were weighed into a test tube, 5 mL of anhydrous ethanol was added and stirred at 10000 rpm for 1 min.

[0067] After the preparation is completed, the mixture is centrifuged at 4000 rpm for 2 min, the supernatant is poured out, and the final precipitate is placed in an oven and dried at 60° C. for about 2 hours to obtain a final powder sample.

[0068] Test conditions: the same as in Example 1.

[0069] Experimental results: Fig.11 Given is ETP2In 1-x Sb x The PLQY curve of Cl5 (x = 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99) with the change of x value shows that in the range of x = 0.05-0.99, the PLQY of the product can always be maintained above 80%. In the range of x = 0.7-0.9, the PLQY reaches nearly 100%, showing the excellent luminescence characteristics of the product of the present invention.

[0070] Matters not covered by the present invention are known technologies.

Claims

1. A yellow phosphor with broadband emission and adjustable spectrum, characterized by The structural formula of the yellow phosphor is ETP2In 1-x Sb x Cl5; Wherein, 0.05≤x≤0.99, and ETP is ethyltriphenylphosphine.

2. The broadband emission and spectrally tunable yellow light phosphor according to claim 1, characterized in that It emits yellow fluorescence under ultraviolet light.

3. The method for preparing the yellow light phosphor with broadband emission and adjustable spectrum as claimed in claim 1, characterized in that the method comprises the following steps: (1) According to the ratio of the above salts, 1-x Sb x According to the corresponding amount ratio of substances in Cl5 (0.05≤x≤0.99), the compound containing ETP, the compound containing In, and the compound containing Sb are added into the container and mixed; in, The ETP-containing compound is a chloride of ETP, namely, ETPCl; the In-containing compound is a chloride or hydrated chloride of In; the Sb-containing compound is a chloride of Sb; (2) adding anhydrous ethanol to the container and stirring at 1000-10000 rpm for 30 seconds to 10 minutes; Wherein, 1-10 mL of anhydrous ethanol was added for every 2 mmol of ETP compound; (3) Centrifuge the product for 1-5 minutes; (4) After centrifugation, the supernatant is poured out, and the final precipitate is dried at 40-80° C. for 2-5 hours to obtain a yellow phosphor with broadband emission and tunable spectrum.

4. The method for preparing the yellow light phosphor with broadband emission and adjustable spectrum as claimed in claim 3, characterized in that The centrifugal speed in step (3) is 3000-5000 rpm.

Citation Information

Patent Citations

  • Antimony pentachloride fluorescent compound, crystal and preparation method and application of antimony pentachloride fluorescent compound