Method for simultaneously preparing titanium slag and vanadium-containing pig iron by taking low-grade vanadium titano-magnetite as raw material

By controlling the feeding method of vanadium titanium magnetite and carbonaceous reducing agent and the power of electric furnace transformer in closed or semi-closed electric furnace, the efficient recovery of iron, vanadium and titanium in vanadium titanium magnetite is solved, and the vanadium content of pig iron is improved , reduces production costs and power consumption, and realizes efficient utilization of resources.

CN119061269APending Publication Date: 2024-12-03冉显俊
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411299445.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently recover iron, vanadium and titanium in vanadium titanium magnetite at the same time, resulting in waste of resources. Especially in low-grade ores, the process is unstable and does not meet safety requirements, making it difficult to increase the vanadium content of pig iron.

Method used

Use a sealed or semi-closed electric furnace to reduce the mixture of low-grade vanadium titanium magnetite and carbonaceous reducing agent in one go or in batches, and control the power and feeding speed of the electric furnace transformer to ensure the separation of titanium slag and vanadium-containing pig iron. Increase the V content of vanadium-containing pig iron to >0.5 wt%.

Benefits of technology

The recycling rate of iron, vanadium and titanium in vanadium titanium magnetite has been greatly improved, the raw material cost and ore dressing cost have been reduced, and the vanadium-containing pig iron that meets market requirements has been stable, reducing power consumption and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a method for preparing titanium slag and vanadium-containing pig iron from low-grade vanadium titano-magnetite, and belongs to the technical field of electric furnace smelting. The invention provides a method for preparing titanium slag and vanadium-containing pig iron from low-grade vanadium titano-magnetite to solve the problems that in the prior art, the vanadium-containing pig iron is low in grade, the requirements for the quality of raw ore and the technical requirements of workers are high, and the requirements for environmental protection and safety are difficult to meet. Comprising the following steps: adding low-grade vanadium titano-magnetite and a carbonaceous reducing agent into a closed or semi-closed electric furnace in batches according to the ratio of 1: (0.2-0.35), and controlling the power of an electric furnace transformer to be 3600-36000 kVA and the temperature of slag water at a slag outlet to be 1650-1780 DEG C to obtain titanium slag and vanadium-containing pig iron. According to the method, the closed or semi-closed electric furnace is adopted, the V in the raw material ore with the extremely low grade can be greatly reduced by controlling the feeding procedure, the using amount of the reducing agent and the furnace charge temperature, it is guaranteed that the V of the vanadium-containing pig iron is larger than 0.5 wt%, and the method is short in technological process, easy to operate, low in cost, clean and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electric furnace smelting titanium slag, and specifically relates to a method for simultaneously preparing titanium slag and vanadium-containing pig iron by taking low-grade vanadium-titanium magnetite as a raw material. Background Art

[0002] Vanadium (V) is a transition metal element. It is widely used in steel, chemical industry, aviation and other fields because of its excellent strength, hardness and anti-fatigue effect. About 84% of vanadium is used in steel as an alloying element and dissolved into steel to form VC and VN, thereby improving the hardness, strength, toughness and wear resistance of steel. Its production products are mainly ferrovanadium. As an important scarce resource in the world, vanadium resources have no vanadium minerals that can be mined alone. Its distribution in nature is very scattered. It is mainly associated with minerals such as vanadium sulfide ore, lead vanadium ore, vanadium dolomite, potassium uranium vanadate ore and vanadium titanomagnetite. Among them, 88% of the world's vanadium is obtained from vanadium titanomagnetite.

[0003] Vanadium-titanium magnetite is a co-existing mineral resource of vanadium, titanium, iron and accompanied by a variety of valuable elements. Titanium, vanadium and iron are the main valuable elements in the mine, and it also contains a variety of beneficial components such as chromium, sulfur, cobalt, nickel, copper, manganese, gallium, scandium and platinum group elements. The mineral resources are not only diverse, but also have good occurrence conditions and high comprehensive utilization value.

[0004] At present, according to the characteristics of their own vanadium-titanium magnetite resources, countries around the world mainly use traditional crushing and grinding-weak magnetic iron separation-flotation titanium separation process technology for the separation and enrichment of vanadium-titanium magnetite. Some countries only select iron but not titanium, and the grade of iron concentrate is TFe≥54%; some countries only select titanium but not iron, and the grade of titanium concentrate is TiO2>45%; and some minerals (vanadium-titanium sub-iron concentrate) are difficult to be selected into titanium concentrate or iron concentrate due to the mineral phase, and are generally used as raw materials for iron smelting. Due to the different properties of ores in different countries, the mineral composition of vanadium-titanium magnetite concentrate obtained by ore dressing is also different, especially the difference in the content of the main beneficial elements vanadium, titanium and iron, which has formed different utilization methods. One is to use it as a raw material for blast furnace ironmaking to recover iron and vanadium; the second is to use it as a raw material for direct reduction in a rotary kiln, and then recover iron and vanadium through melting and reduction in an electric furnace; the third is that the TiO2 content in the concentrate is very high, and it is used as a raw material for electric furnace smelting high-titanium slag, the main purpose is to recover titanium, and iron is recovered as a by-product. Regardless of the purpose, the efficient recycling of iron, vanadium and titanium in vanadium-titanium magnetite has not been achieved, resulting in a waste of resources. Currently, especially in the production of titanium dioxide and sponge titanium, vanadium as a harmful element is treated as an "impurity" and discarded.

[0005] CN114164310B discloses a method for smelting vanadium-containing pig iron with vanadium slag and acid-soluble titanium slag without adding desulfurized slag material lime. For a closed electric furnace, especially a large electric furnace above 25000KVA, it is difficult to spread the carbonaceous reducing agent on the bottom of the submerged arc furnace. In addition, due to the physical properties of vanadium-titanium magnetite, it is difficult to achieve submerged arc smelting.

[0006] CN109943719A discloses a method for preparing titanium slag and vanadium-containing pig iron simultaneously with vanadium-titanium magnetite as raw material, comprising the following steps: adding vanadium-titanium magnetite and carbonaceous reducing agent in a weight ratio of 1:0.2-0.35 to an electric furnace for reduction, and then performing slag-iron separation to obtain titanium slag and vanadium-containing pig iron. In practice, the inventor found that the titanium slag obtained by the method has a high V2O5 content, resulting in a low recovery rate of V in pig iron, and the vanadium content in each furnace of molten iron is affected by many factors (such as the amount of carbon added, the timing of carbon addition, etc.), the process is unstable, and the qualified rate of vanadium-containing pig iron products is low. At the same time, due to the increasingly stringent environmental protection and safety requirements in recent years, the addition of bottom carbon to an empty furnace and the addition of carbon to strengthen reduction in the later stage of smelting can no longer be operated on the furnace platform, which does not meet the safety requirements (requiring workers to stay away from the furnace platform and remotely operate and control). Furthermore, the original national standard FO2-FO5 for vanadium-containing pig iron (i.e., 0.2%-0.5% vanadium in molten iron) has been eliminated by the market. The vanadium content of vanadium-containing pig iron currently recognized by the market is >0.5%, which places extremely high demands on the selection of titanium and vanadium contents in the raw ore and the technical level of the operators, and is not conducive to the industrial utilization of low-grade ore.

[0007] Therefore, it is necessary to develop a new process suitable for low-grade vanadium-titanium magnetite to increase the vanadium content of pig iron. Summary of the invention

[0008] The object of the present invention is to provide a method for simultaneously recycling iron, vanadium and titanium in vanadium-titanium magnetite, especially low-grade vanadium-titanium magnetite, and to increase the vanadium content in pig iron.

[0009] To achieve the above-mentioned purpose, the present invention provides a method for simultaneously preparing titanium slag and vanadium-containing pig iron using low-grade vanadium-titanium magnetite as raw material, which comprises the following steps: loading a mixture of low-grade vanadium-titanium magnetite and a carbonaceous reducing agent in a weight ratio of 1:0.2-0.35 into a hopper at the top of a closed or semi-closed electric furnace at one time, adding the mixture into the closed or semi-closed electric furnace in batches through a corresponding transverse screw feeder below the hopper for reduction, controlling the power of the electric furnace transformer to be 3600-36000 kVA, continuing the reduction after the addition of materials, separating slag from iron after the reduction is completed, controlling the slag water temperature at the slag outlet to be 1650-1780°C, and obtaining titanium slag and vanadium-containing pig iron; V in the vanadium-containing pig iron is greater than 0.5wt%.

[0010] Wherein, in the above method, the low-grade vanadium-titanium magnetite is at least one of iron concentrate, titanium concentrate, vanadium-titanium subiron ore or vanadium-iron subiron ore.

[0011] Preferably, in the above method, the low-grade vanadium-titanium magnetite is at least one of vanadium-titanium ferrite or vanadium-iron ferrite.

[0012] In the above method, the iron concentrate has a TFe content of 54-62wt%, TiO2 of 8-18wt%, and V2O5 of 0.3-2.0wt%; the titanium concentrate has a TFe content of 30-40wt%, TiO2 of 45-50wt%, and V2O5 of 0.3-2.0wt%; the vanadium-titanium sub-iron ore has a TFe content of 40-54wt%, TiO2 of 16-32wt%, and V2O5 of 0.3-2.0wt%; the vanadium-iron sub-titanium ore has a TFe content of 28-40wt%, TiO2 of 32-45wt%, and V2O5 of 0.3-2.0wt%.

[0013] Preferably, in the above method, the V2O5 content in the low-grade vanadium-titanium magnetite is 0.3-0.44 wt%, and the total amount of titanium iron (i.e., the weight proportion of TiO2+iron and iron oxides) is ≥ 75 wt%.

[0014] Among them, in the above method, the specific manner of adding in batches is: the mixture is added to the electric furnace in 3 to 5 batches, and there is an interval of 0.5 to 1 hour after each batch of feeding is completed. The feeding speed of the first batch is controlled to be 300 to 400 kg / minute, and the feeding speed of each subsequent batch is controlled to be 150 to 200 kg / minute; or the mixture is added to the electric furnace in 2 batches, and the feeding speed of the first batch is controlled to be 300 to 400 kg / minute. The feeding amount of the first batch is 1 / 4 of the total material. After the first batch of feeding is completed, there is an interval of 0.5 to 1 hour, and the second batch is continuously fed. The feeding amount of the second batch is 3 / 4 of the total material, and the feeding speed of the second batch is controlled to be 65 to 75 kg / minute.

[0015] Among them, in the above method, the time for continued reduction after adding the materials is controlled to be no less than 1 hour, and the full-load power supply time is controlled to be 6 to 7 hours.

[0016] Preferably, in the above method, the power of the electric furnace transformer is controlled to be 6300-33000 kVA.

[0017] Preferably, in the above method, the slag water temperature at the slag outlet is controlled to be 1680-1720°C.

[0018] Wherein, in the above method, the carbonaceous reducing agent is at least one of diced, granular or powdered coke, blue carbon, anthracite and petroleum coke; the fixed carbon of the carbonaceous reducing agent is 80-95wt%.

[0019] Among them, in the above method, the titanium slag is sprayed with water immediately after it comes out of the furnace to quickly cool it down to below 850°C, and the TiO2 in the obtained titanium slag is ≥70wt%.

[0020] Beneficial effects of the present invention:

[0021] The present invention uses vanadium-titanium sub-iron ore or vanadium-iron sub-titanium ore as raw material to produce titanium slag, which greatly reduces the requirements for raw materials used in titanium slag production and greatly expands the selection range of raw material ore. The present invention first adds the one-time batching into the corresponding hopper above the screw conveyor, and then adds it into a closed or semi-closed electric furnace in batches, and isolates air from entering the electric furnace as much as possible. At the same time, by controlling the amount of carbonaceous reducing agent and the temperature of the charge in the furnace, V2O5 in the low-grade vanadium-titanium magnetite is greatly reduced and enters the molten iron, so that the byproduct semi-steel is converted into vanadium-containing pig iron, ensuring that V in the vanadium-containing pig iron is greater than 0.5wt%, and the added value is increased. The present invention can also shorten the entire reaction time and the thoroughness of reduction by controlling the voltage of the electric furnace transformer, thereby further saving costs. DETAILED DESCRIPTION

[0022] Specifically, a method for simultaneously preparing titanium slag and vanadium-containing pig iron using low-grade vanadium-titanium magnetite as raw material comprises the following steps: loading a mixture of low-grade vanadium-titanium magnetite and a carbonaceous reducing agent in a weight ratio of 1:0.2-0.35 into a hopper on the top of a closed or semi-closed electric furnace at one time, adding the mixture in batches into the closed or semi-closed electric furnace for reduction through a corresponding screw feeder under the hopper, controlling the power of the electric furnace transformer to be 3600-36000 kVA, continuing the reduction after the addition of materials, separating slag from iron after the reduction, controlling the slag water temperature at the slag outlet to be 1650-1780°C, and obtaining titanium slag and vanadium-containing pig iron; V>0.5wt% in the vanadium-containing pig iron.

[0023] In the method of the present invention, the vanadium-titanium magnetite can be at least one of iron concentrate, titanium concentrate, vanadium-titanium iron ore or vanadium-iron iron ore. When the vanadium-titanium iron ore or vanadium-iron iron ore is used as a raw material to produce titanium slag, the raw material cost can be greatly reduced, and the direct utilization rate of the vanadium-titanium iron ore or vanadium-iron iron ore can be improved, and the washing cost during ore dressing can be greatly reduced.

[0024] In the method of the present invention, the iron concentrate contains 54-62wt% TFe, 8-18wt% TiO2 and 0.3-2.0wt% V2O5; the titanium concentrate contains 30-40wt% TFe, 45-50wt% TiO2 and 0.3-2.0wt% V2O5; the vanadium-titanium ore contains 40-54wt% TFe, 18-32wt% TiO2 and 0.3-2.0wt% V2O5; the vanadium-iron ore contains 28-40wt% TFe, 32-45wt% TiO2 and 0.3-2.0wt% V2O5.

[0025] The present invention preferably uses a closed electric furnace to efficiently recycle coal gas. If a semi-closed furnace is used, all charging furnace doors and observation holes should be closed, and an overhead automatic charging system should be used. Otherwise, multiple charging will cause part of the fine-grained carbon and part of the coarse-grained carbon surface to directly burn with oxygen in the air, which will not achieve a full reduction effect and waste the carbonaceous reducing agent. For a semi-closed furnace, if a one-time charging is used, due to the strong disturbance of the electric arc in the furnace, part of the fine-grained carbonaceous reducing agent will be sucked away by a large-flow exhaust gas fan and burned in the middle and upper part of the furnace and the flue, which will also cause waste. Therefore, for a semi-closed furnace, in addition to taking necessary sealing measures (oxygen content in the exhaust gas <16%), it is also necessary to significantly reduce the exhaust gas fan flow rate and significantly reduce the cold air entering the furnace, thereby significantly reducing heat energy loss and oxygen content in the furnace, while reducing the labor intensity of workers and reducing excessive dependence on workers' operating level.

[0026] Due to the airtightness and safety requirements of electric furnaces, it is extremely difficult to add bottom carbon to an empty furnace and add carbon to strengthen reduction in the later stage of smelting. Therefore, it is necessary to add a sufficient amount of carbonaceous reducing agent at one time in the batching process and mix the materials evenly to ensure that the metal oxides (including multivalent oxides) such as iron and vanadium in the raw ore can be basically reduced. If an excessive amount of carbonaceous reducing agent is added, the C in the pig iron will increase, increasing the production cost. The inventor of the present invention has conducted a large number of experiments and found that only under the dosage and temperature control of the carbonaceous reducing agent of the present invention can qualified titanium slag be obtained with low-grade vanadium-titanium magnetite as raw material, and vanadium-containing pig iron that meets market requirements (V>0.5wt%) can be stably obtained.

[0027] In the molten pool in the furnace, the farther away from the electrode, the lower the temperature. In order to ensure the reduction effect, the low temperature point in the molten pool must be higher than 1640°C. For this reason, to be on the safe side, it is better to control the temperature of the melt in the molten pool in the furnace at about 1710°C. If the temperature is too high, the power consumption will be too large, and the life of the furnace will be greatly shortened, causing safety hazards. Since the present invention adopts a closed or semi-closed electric furnace, it is difficult to monitor the temperature of the molten pool in the furnace. Therefore, the present invention indirectly controls the temperature of the molten pool in the furnace by controlling the temperature of the slag water at the slag outlet. Generally, the temperature of the slag water at the slag outlet is 20 to 60°C lower than the temperature of the molten pool in the furnace; therefore, the present invention controls the temperature of the slag water at the slag outlet to 1650 to 1780°C; preferably 1680 to 1720°C.

[0028] The inventors found in actual production that when the V2O5 content in the raw material ore is high, the process of CN109943719A can be used to obtain vanadium-containing pig iron with V>0.5wt%. However, there are the following problems:

[0029] 1. Due to the high oxygen concentration in the air in the furnace, the V2O5 content in the titanium slag is too high and is not fully reduced, resulting in a low V recovery rate, which reduces the value of vanadium-containing pig iron (the higher the V content in the pig iron, the more expensive it is).

[0030] 2. The quality of vanadium-containing pig iron is unstable due to the great influence of workers' operating level, which also reduces the value of vanadium-containing pig iron.

[0031] 3. The production cost is too high, especially the electricity consumption per ton of slag will increase by more than 2,000 degrees.

[0032] When the process of CN109943719A is used, it is difficult to stably obtain vanadium-containing pig iron with V>0.5wt% when the V2O5 content in the raw material ore is low. Therefore, when the total amount of ferrotitanium in the raw material ore remains unchanged, this process reduces the high requirement for the V2O5 content in the raw material ore and broadens the range of raw material selection.

[0033] In the method of the present invention, the specific manner of adding in batches is: the mixed material is added to the electric furnace in 3 to 5 batches, and each batch is added with an interval of 0.5 to 1h after the addition is completed, the first batch of feeding speed is controlled to be 300 to 400kg / minute, and the subsequent feeding speed of each batch is controlled to be 150 to 200kg / minute; or the mixed material is added to the electric furnace in 2 batches, the first batch of feeding speed is controlled to be 300 to 400kg / minute, the first batch of feeding amount is 1 / 4 of the total material, and after the first batch of feeding is completed, the second batch of continuous feeding is performed with an interval of 0.5 to 1h, the second batch of feeding amount is 3 / 4 of the total material, and the second batch of feeding speed is controlled to be 65 to 75kg / minute. By accurately controlling the feeding time and feeding speed in stages, the molten pool in the furnace does not "turn over slag", which is more conducive to vanadium reduction, and then stably obtains vanadium-containing pig iron that meets market requirements (V>0.5wt%), and can save raw and auxiliary materials, reduce power consumption, and save costs.

[0034] In the method of the present invention, the time for continued reduction after adding the materials is controlled to be no less than 1 hour, and the full-load power transmission time is controlled to be 6 to 7 hours.

[0035] The higher the content of fixed carbon in the carbonaceous reducing agent, the less the impurity content, and the better the reducing performance; the lower the fixed carbon content, the higher the impurity content, which will affect the grade of the final titanium slag. Therefore, in the method of the present invention, the carbonaceous reducing agent used is at least one of diced, granular or powdered coke, blue carbon, anthracite, and petroleum coke; the fixed carbon of the carbonaceous reducing agent is 80-95wt%.

[0036] The present invention can shorten the reaction time and save costs by controlling the voltage of the electric furnace transformer. Since the power of different electric furnace transformers is different, the corresponding voltage is also different. In the technical field of the present invention, the power of the electric furnace transformer can be 3600-36000 kVA and it is best to be a closed electric furnace; the power of the electric furnace transformer is preferably 6300-33000 kVA. In the actual operation process, if the power of the electric furnace transformer is not within the scope of the present invention, the corresponding voltage can be adjusted according to the actual situation, as long as the temperature in the furnace can be effectively controlled and the reaction time can be shortened.

[0037] In the present invention, the titanium slag should be sprayed with water or immersed in water immediately after it is taken out of the furnace to quickly cool it to below 850°C to reduce the generation of rutile. In the present invention, the TiO2 in the obtained titanium slag is ≥70wt%.

[0038] Before the molten iron is discharged from the furnace, its temperature should be reduced to about 1400℃, which is the standard for not sticking to the mold. After the molten iron is discharged from the furnace, it enters the ladle through the chute or enters the cast iron machine to be directly cast into block-shaped vanadium-containing pig iron, which becomes the raw material for oxygen blowing and vanadium extraction slag in the subsequent process; or, if the sulfur, phosphorus and other elements in the molten iron are well controlled by ore blending, it can be directly used as a vanadium additive for the refined molten iron of rebar, replacing high-vanadium iron and reducing the production cost of rebar.

[0039] The specific implementation of the present invention is further described below in conjunction with the embodiments, but the present invention is not limited to the scope of the embodiments. At the same time, a series of improvements and improvement measures can be made without violating the principles of the present invention, and these measures should also be included in the protection scope of the present invention.

[0040] Example 1

[0041] According to Table 1, vanadium-titanium iron ore and coke powder are prepared into a mixture, loaded into 6 hoppers placed around the furnace top, and added into a 6300KVA semi-enclosed electric furnace through the corresponding horizontal screw feeder under each hopper. The mixture is added in 4 times (7 tons each time). The first batch feeding speed is 350kg / min (feeding takes 20 minutes), and the subsequent feeding speed is 175kg / min (each batch takes 40 minutes). Each feeding is completed after an interval of 1 hour before the next feeding. During the smelting period, the voltage of the electric furnace transformer is adjusted to supply power at high load, and the power of the electric furnace transformer is controlled to 6300KVA. After the feeding is completed, smelting continues for 1 hour and 20 minutes. The total full-load power supply smelting time is about 6.5 hours.

[0042] After the power is turned off, the titanium slag is discharged first, and the slag water temperature at the slag outlet is 1700℃. After the titanium slag is discharged from the furnace, the surface is quickly sprayed with water to cool down to below 850℃ to reduce the production of rutile. After the slag is discharged and the slag outlet is sealed, the 6 horizontal screw feeders placed around the furnace top are quickly started and about 7 tons of mixed materials are added to the furnace at the same time (this is the first charging of the next furnace) to cool the molten iron in the furnace to 1450℃. At the same time, the newly added raw material ore absorbs heat and heats up rapidly. The molten iron is discharged from the iron outlet to obtain vanadium-containing pig iron. After the iron outlet is sealed, power is immediately supplied for the smelting of the next furnace. The second charging is carried out 40 minutes later, with a charging speed of 175kg / minute, and so on for the third and fourth charging; or continuous charging is carried out after 40 minutes, with a charging speed of 65-75kg / minute.

[0043] The quality of the obtained titanium slag and vanadium-containing pig iron is shown in Table 1.

[0044] Table 1 Unit: wt%

[0045]

[0046] As can be seen from Table 1, qualified titanium slag and qualified vanadium-containing pig iron were prepared using vanadium-titanium sub-iron ore with low titanium content as raw material. V2O5 in the raw ore has been largely reduced to V and enters the molten iron.

[0047] Example 2

[0048] According to Table 2, vanadium iron ore and coke powder are prepared into a mixture, loaded into 6 hoppers placed around the furnace top, and added into a 6300KVA semi-enclosed electric furnace through the corresponding horizontal screw feeder under each hopper. The mixture is added in 4 times (7 tons each time). The first batch feeding speed is 350kg / min (feeding takes 20 minutes), and the subsequent feeding speed is 175kg / min (each batch takes 40 minutes). Each feeding is completed with an interval of 40 minutes before the next feeding. During the smelting period, the voltage of the electric furnace transformer is adjusted to supply power at high load, and the power of the electric furnace transformer is controlled to 6300KVA. After the feeding is completed, smelting continues for 2 hours and 20 minutes, and the total full-load power supply smelting time is about 6.5 hours.

[0049] After the power is turned off, the titanium slag is discharged first, and the slag water temperature at the slag outlet is 1700℃. After the titanium slag is discharged from the furnace, the surface is quickly sprayed with water to cool down to below 850℃ to reduce the production of rutile. After the slag is discharged and the slag outlet is sealed, the 6 horizontal screw feeders placed around the furnace top are quickly started and about 7 tons of raw ore are added to the furnace at the same time (this is the first charging of the next furnace) to cool the molten iron in the furnace to 1450℃. At the same time, the newly added raw ore absorbs heat and heats up rapidly. The molten iron is discharged from the iron outlet to obtain vanadium-containing pig iron. After the iron outlet is sealed, power is immediately supplied for the smelting of the next furnace. The second charging is carried out 1 hour later, with a charging speed of 175kg / minute, and the third and fourth charging are carried out by analogy; or continuous charging is carried out after 40 minutes, with a charging speed of 65-75kg / minute.

[0050] The quality of the obtained titanium slag and vanadium-containing pig iron is shown in Table 2.

[0051] Table 2 Unit: wt%

[0052]

[0053] As can be seen from Table 2 above, qualified titanium slag and qualified vanadium-containing pig iron were prepared simultaneously using sub-titanium ore with low iron and vanadium contents as raw materials. Compared with Example 2 of CN109943719A, the V grade in the vanadium-containing pig iron was increased to > 0.5%wt%, the qualified rate of vanadium-containing pig iron was greatly improved, and the power consumption per ton of slag was reduced by about 2500 degrees or more, meeting the new market requirements for qualified vanadium-containing pig iron.

[0054] Comparative Example 1

[0055] First, add 20kg / ton of coke powder to the empty titanium slag electric furnace; then, mix the vanadium-titanium iron concentrate and coke powder in a weight ratio of 1:0.16 and put them into the titanium slag electric furnace; adjust the secondary output voltage of the electric furnace transformer (power is 3200kVA) to the lowest level of 135V; after power-on, the primary current slowly increases from 80A to 180A until it is discharged from the furnace 3 hours later; add coke powder twice, 15kg / ton of ore each, 1 hour and half an hour before discharge; after the furnace charge is separated, titanium slag and vanadium-containing pig iron are obtained; the titanium slag after discharge is quickly sprayed with water to cool down to below 850℃. The quality of the obtained titanium slag and vanadium-containing pig iron is shown in Table 3.

[0056] Table 3 Unit: wt%

[0057]

[0058] It can be seen from Table 3 above that, compared with Example 2, by using the method of CN109943719A, the V2O5 content in the titanium slag obtained is relatively high, the V content in the vanadium-containing pig iron is relatively low, and the vanadium-containing pig iron with V>0.5wt% cannot be obtained.

[0059] Example 3

[0060] According to Table 4, vanadium-titanium sub-iron ore and coke powder are prepared into a mixture, loaded into 6 hoppers placed around the furnace top, and added into a 6300KVA semi-enclosed electric furnace through the corresponding horizontal screw feeder under each hopper. The mixture is added in 4 times (7 tons each time). The first batch feeding speed is 350kg / min (feeding takes 20 minutes), and the subsequent feeding speed is 175kg / min (each batch takes 40 minutes). Each feeding is completed with an interval of 1 hour before the next feeding. During the smelting period, the voltage of the electric furnace transformer is adjusted to supply power at a high load, and the power of the electric furnace transformer is controlled to be 6300KVA. After the feeding is completed, smelting continues for 1 hour and 20 minutes. The total full charge power supply smelting time is about 6.5 hours.

[0061] After the power is turned off, the titanium slag is discharged first, and the slag water temperature at the slag outlet is 1700℃. After the titanium slag is discharged from the furnace, the surface is quickly sprayed with water to cool down to below 850℃ to reduce the production of rutile. After the slag is discharged and the slag outlet is sealed, the 6 horizontal screw feeders placed around the furnace top are quickly started and about 7 tons of raw ore are added to the furnace at the same time (this is the first charging of the next furnace) to cool the molten iron in the furnace to 1450℃. At the same time, the newly added raw ore absorbs heat and heats up rapidly. The molten iron is discharged from the iron outlet to obtain vanadium-containing pig iron. After the iron outlet is sealed, power is immediately supplied for the smelting of the next furnace. The second charging is carried out 40 minutes later, with a charging speed of 175kg / min, and so on for the third and fourth charging; or continuous charging is carried out after 40 minutes, with a charging speed of 65-75kg / min.

[0062] The quality of the obtained titanium slag and vanadium-containing pig iron is shown in Table 4.

[0063] Table 4 Unit: wt%

[0064]

[0065] It can be seen from Table 4 that the titanium slag and vanadium-containing pig iron are of qualified quality when the vanadium-titanium sub-iron ore with low titanium content is used as raw material. Compared with Example 1 of CN109943719A, the V2O5 in the raw material ore has been largely reduced to V and enters the molten iron. In addition, the vanadium content of the vanadium-containing pig iron is relatively stable, which is greatly reduced by the technical level of the operators, greatly improving the qualified rate of the vanadium-containing pig iron; at the same time, the power consumption per ton of slag is reduced by about 2500 degrees, which is more conducive to large-scale industrial production.

[0066] Comparative Example 2

[0067] First, add 20kg / ton of coke powder to the empty titanium slag electric furnace; then, mix the vanadium-titanium iron concentrate and coke powder in a weight ratio of 1:0.18, and then put them into the titanium slag electric furnace; adjust the secondary output voltage of the electric furnace transformer (power is 3200kVA) to the lowest gear 135V; after power-on, the primary current is slowly increased from 80A to 180A until it is discharged from the furnace 3 hours later; 15kg / ton of coke powder is added twice 1 hour and half an hour before discharge; after the furnace charge is separated after discharge, titanium slag and vanadium-containing pig iron are obtained; after discharge, the titanium slag is quickly sprayed with water to cool down to below 850℃, and rutile is produced as little as possible. The quality of the obtained titanium slag and vanadium-containing pig iron is shown in Table 5.

[0068] Table 5 Unit: wt%

[0069]

[0070] It can be seen from Table 5 that when using vanadium-titanium sub-iron ore with a low titanium content as raw material and adopting the CN109943719A method, the V2O5 content in the slag is too high and not fully reduced.

[0071] Comparative Example 3

[0072] According to Table 6, vanadium-titanium sub-iron ore and coke powder are prepared into a mixture, loaded into 6 hoppers placed around the furnace top, and added into a 6300KVA semi-enclosed electric furnace through the corresponding horizontal screw feeder under each hopper. The mixture is added in 4 times (7 tons each time). The first batch feeding speed is 350kg / min (feeding takes 20 minutes), and the subsequent feeding speed is 175kg / min (each batch takes 40 minutes). Each feeding is completed with an interval of 1 hour before the next feeding. During the smelting period, the current at the output end of the electric furnace transformer is adjusted to 85% to 90% load, and the power of the electric furnace transformer is controlled to be about 5500KVA. After the feeding is completed, smelting continues for 1 hour and 20 minutes, and the total power supply smelting time is about 6.5 hours.

[0073] After the power is turned off, the titanium slag is discharged first, and the slag water temperature at the slag outlet is 1580℃. After the titanium slag is discharged from the furnace, water is sprayed on the surface to cool it down to below 850℃ to reduce the generation of rutile. The molten iron is discharged from the iron outlet to obtain vanadium-containing pig iron.

[0074] Table 6 Unit: wt%

[0075]

[0076] It can be seen from Table 6 that when using vanadium-iron titanite with low iron and vanadium contents as raw material, when the reduction temperature is low, although the iron oxide in the titanium slag is basically reduced, the V2O5 is basically not completely reduced.

[0077] Comparative Example 4

[0078] According to Table 7, vanadium iron ore and coke powder are prepared into a mixture, loaded into 6 hoppers placed around the furnace top, and added into a 6300KVA semi-closed electric furnace through the corresponding horizontal screw feeder under each hopper. The mixture is added in 4 times (7 tons each time). The first batch feeding speed is 350kg / min (feeding takes 20 minutes), and the subsequent feeding speed is 175kg / min (each batch takes 40 minutes). Each feeding is completed with an interval of 40 minutes before the next feeding. During the smelting period, the voltage of the electric furnace transformer is adjusted to supply power at a high load, and the power of the electric furnace transformer is controlled to be 6300KVA. After the feeding is completed, smelting continues for 2 hours and 20 minutes. The total full charge power supply smelting time is about 6.5 hours.

[0079] After the power is turned off, the titanium slag is discharged first, and the slag water temperature at the slag outlet is 1700℃. After the titanium slag is discharged from the furnace, water is sprayed on the surface to cool it down to below 850℃ to reduce the generation of rutile. The molten iron is discharged from the iron outlet to obtain vanadium-containing pig iron.

[0080] The quality of the obtained titanium slag and vanadium-containing pig iron is shown in Table 7.

[0081] Table 7 Unit: wt%

[0082]

[0083] As can be seen from Table 7, since the complete reduction temperature of iron oxide is much lower than that of V2O5, the carbon in the furnace first undergoes a reduction reaction with the iron oxide, and only when the temperature is appropriate can the remaining carbon undergo a complete reduction reaction with V2O5. Therefore, when using vanadium-iron sub-titanium ore with low iron and vanadium content as raw material, when the amount of coke powder is insufficient, the V2O5 in the titanium slag is not completely reduced, the metal vanadium content in the pig iron is insufficient, and the vanadium-containing pig iron is unqualified.

Claims

1. A method for simultaneously preparing titanium slag and vanadium-containing pig iron using low-grade vanadium-titanium magnetite as raw material, characterized in that: The method comprises the following steps: loading a mixture of low-grade vanadium-titanium magnetite and a carbonaceous reducing agent in a weight ratio of 1:0.2-0.35 into a hopper on the top of a closed or semi-closed electric furnace at one time, adding the mixture into the closed or semi-closed electric furnace in batches through a corresponding screw feeder under the hopper for reduction, controlling the power of the electric furnace transformer to be 3600-36000 kVA, continuing the reduction after the feeding is completed, separating slag from iron after the reduction is completed, controlling the temperature of slag water at a slag outlet to be 1650-1780°C, and obtaining titanium slag and vanadium-containing pig iron; wherein V in the vanadium-containing pig iron is greater than 0.5wt%.

2. The method according to claim 1, characterized in that: The low-grade vanadium-titanium magnetite is at least one of iron concentrate, titanium concentrate, vanadium-titanium ferrite or vanadium-iron ferrite; preferably, the low-grade vanadium-titanium magnetite is at least one of vanadium-titanium ferrite or vanadium-iron ferrite.

3. The method according to claim 2, characterized in that: The iron concentrate contains 54-62wt% TFe, 8-18wt% TiO2 and 0.3-2.0wt% V2O5; the titanium concentrate contains 30-40wt% TFe, 45-50wt% TiO2 and 0.3-2.0wt% V2O5; the vanadium-titanium ore contains 40-54wt% TFe, 16-32wt% TiO2 and 0.3-2.0wt% V2O5; the vanadium-iron ore contains 28-40wt% TFe, 32-45wt% TiO2 and 0.3-2.0wt% V2O5.

4. The method according to any one of claims 1 to 3, characterized in that: The low-grade vanadium-titanium magnetite contains 0.3-0.44 wt% of V2O5 and the total amount of ferrotitanium is ≥75 wt%.

5. The method according to claim 1, characterized in that: The specific method of adding in batches is: the mixed material is added to the electric furnace in 3 to 5 batches, and there is an interval of 0.5 to 1 hour after each batch of feeding is completed. The feeding speed of the first batch is controlled to be 300 to 400 kg / minute, and the feeding speed of each subsequent batch is controlled to be 150 to 200 kg / minute; or the mixed material is added to the electric furnace in 2 batches, and the feeding speed of the first batch is controlled to be 300 to 400 kg / minute. The feeding amount of the first batch is 1 / 4 of the total material. After the first batch of feeding is completed, there is an interval of 0.5 to 1 hour, and the second batch is continuously added. The feeding amount of the second batch is 3 / 4 of the total material, and the feeding speed of the second batch is controlled to be 65 to 75 kg / minute.

6. The method according to claim 1, characterized in that: The reduction time after adding materials should be controlled to be no less than 1 hour, and the full load power supply should be controlled to be 6 to 7 hours.

7. The method according to claim 1, characterized in that: The power of the electric furnace transformer is controlled from 6300 to 33000 kVA.

8. The method according to claim 1, characterized in that: Control the slag water temperature at the slag outlet to 1680~1720℃.

9. The method according to claim 1, characterized in that: The carbonaceous reducing agent is at least one of diced, granular or powdered coke, blue carbon, anthracite and petroleum coke; the fixed carbon of the carbonaceous reducing agent is 80-95wt%.