High-aluminum dispersion copper alloy material and preparation method thereof

By doping aluminum and trace metal elements in high-aluminum diffused copper alloy, combined with water atomization method and thermal isostatic pressing process, the problem of incomplete internal oxidation is solved, and the hardness, conductivity and elongation of the material are significantly improved. , meets the high-performance market demand.

CN119061286APending Publication Date: 2024-12-03ZHUZHOU SMELTER GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972387.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

There is a trend of aluminum in the internal oxidation process in the existing high-aluminum diffusion copper alloy materials, resulting in incomplete internal oxidation, and the performance of material hardness, conductivity and other properties are limited, making it difficult to meet the high-performance needs in new energy batteries, welding and other fields. .

Method used

By doping a certain amount of aluminum elements and metal elements with trace reduction properties in copper, water atomization method is used to prepare copper alloy powder, and sintering and internal oxidation are combined with cold isostatic pressure and hot isostatic pressure processes. Subsequently, it is reduced in a hydrogen atmosphere and finally heat extrusion treatment is performed to form a high-aluminum diffused copper alloy material with high hardness, wear resistance, conductivity and elongation.

Benefits of technology

The high-strength, wear resistance, conductivity and elongation of high-aluminum diffused copper alloy materials have been achieved, with density ≥8.75g/cm3, hardness ≥70HRB, conductivity ≥70% IACS, tensile strength ≥400MPa, elongation ≥10%, meeting the broader market application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061286A_ABST
    Figure CN119061286A_ABST
Patent Text Reader

Abstract

The invention provides a high-aluminum dispersion copper alloy material which comprises the following components in percentage by mass: 0.4-2.0 wt% of Al, 0.1-2.0 wt% of metal of which the reducibility is lower than that of aluminum, less than 0.3 wt% of oxygen content and the balance of Cu and inevitable impurities. The invention provides a preparation method of a high-aluminum dispersion copper alloy material. According to the preparation method of the high-aluminum dispersion copper alloy material, the prepared high-aluminum dispersion copper alloy material has the excellent performance of high strength and hardness, high wear resistance, high conductivity and high elongation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal matrix composite materials, and in particular to a method for preparing a high-aluminum dispersed copper alloy material. Background Art

[0002] Alumina dispersed copper alloy has excellent high-temperature properties such as high strength, high hardness, high conductivity and high softening temperature, and has broad market application prospects in rail transportation, aerospace, automobile and other fields.

[0003] At present, many studies have been conducted on the preparation process of high-performance alumina dispersed copper alloys at home and abroad in order to obtain dispersed copper alloys with excellent performance. In Europe and the United States, alumina dispersed copper alloys prepared by internal oxidation have formed an electrode material industry chain. Among them, the alumina dispersed copper alloys of grades C15715, C15740 and C15760 produced by SCM in the United States using internal oxidation have a daily production scale of 20 tons. The alumina dispersed copper alloy products produced by domestic enterprises such as Guangzhou Nonferrous Metals, China Aluminum Luoyang Copper, and China Shipbuilding Industry Corporation are all concentrated in low-aluminum dispersed copper alloys.

[0004] However, the welding of new energy batteries, aluminum alloys, high-strength steel, galvanized plates, nickel-plated plates and other materials requires high quality and is difficult. In addition, other application scenarios also place higher demands on the hardness, strength, wear resistance and other properties of the materials. Therefore, high-aluminum dispersed copper alloy products with better performance are currently needed.

[0005] Generally, the reverse diffusion trend of aluminum increases during the internal oxidation of high-aluminum dispersed copper, resulting in the formation of a continuous internal oxide film inside the material, which hinders the further occurrence of internal oxidation and leads to incomplete internal oxidation. In addition, due to the high concentration of solute elements, A12O3 particles are easy to grow during the internal oxidation process, which inhibits the strengthening effect and affects the hardness, conductivity and other properties of the material, limiting the application of high-aluminum dispersed copper alloy materials.

[0006] Therefore, there is an urgent need for a high-aluminum dispersed copper alloy material with high strength, hardness, wear resistance, conductivity and elongation, so that the high-aluminum dispersed copper alloy material can meet the needs of a wider market application. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a high-aluminum dispersed copper alloy material with high hardness, high wear resistance, high conductivity and high elongation and a preparation method thereof.

[0008] To solve the above technical problems, the present invention provides a high-aluminum dispersed copper alloy material, which includes, by mass percentage, 0.4-2.0wt% Al, 0.1-2.0wt% metal with lower reducibility than aluminum, oxygen content <0.3wt%, and the remainder Cu and unavoidable impurities.

[0009] Furthermore, the metal having a lower reducing property than aluminum is one or more of Ti, Ag, Ni, Sn, Cr, Zr and Zn.

[0010] The present invention also provides a method for preparing a high-aluminum dispersed copper alloy material, comprising the following steps:

[0011] Copper, aluminum and a metal with a lower reducing power than aluminum are mixed and smelted, and after smelting, a copper alloy powder containing 0.4-2.0wt% of Al, 0.1-2.0wt% of a metal with a lower reducing power than aluminum, less than 0.3wt% of oxygen, and the remainder being Cu and unavoidable impurities is prepared by water atomization method;

[0012] The copper alloy powder is mixed with an oxidant and then cold isostatically pressed to obtain a copper alloy blank;

[0013] The copper alloy blank is sealed by encapsulation, and then hot isostatically pressed to obtain a high-aluminum dispersed copper alloy ingot after vacuuming.

[0014] The high aluminum dispersed copper alloy ingot is unwrapped and reduced in a hydrogen atmosphere;

[0015] hot-extrude the reduced high-aluminum dispersed copper alloy ingot to obtain a high-aluminum dispersed copper alloy material doped with trace elements;

[0016] Wherein, the metal with lower reducing property than aluminum is one or more of Ti, Ag, Ni, Sn, Cr, Zr and Zn.

[0017] Furthermore, the smelting temperature during smelting is 1100° C.-1250° C., and the particle size of the copper alloy powder is less than 60 mesh.

[0018] Furthermore, the oxidant is Cu2O powder, and the particle size of the Cu2O powder is less than 500 meshes.

[0019] Furthermore, the cold isostatic pressing adopts a polyurethane mold, and the cold isostatic pressing pressure is 150-300 MPa.

[0020] Furthermore, the temperature of the copper alloy blank after the vacuum is evacuated after the sheath is sealed is 500°C.

[0021] -600℃, time ≥10h, vacuum degree less than 5×10 -3 Pa.

[0022] Furthermore, the hot isostatic pressing pressure is 30-200 MPa, the hot isostatic pressing temperature is 500° C.-1000° C., and the hot isostatic pressing time is 1-8 h.

[0023] Furthermore, the reduction temperature in the hydrogen atmosphere is 50-900° C., and the reduction time is 1-16 hours.

[0024] Furthermore, the extrusion temperature during the hot extrusion is 700-950° C., and the extrusion ratio is 10-50.

[0025] The present invention provides a high-aluminum dispersed copper alloy material, in which a certain amount of aluminum element is doped into copper to form alumina dispersed copper, and at the same time a trace amount of metal element with a lower reducibility than aluminum is doped into the copper, and the trace metal element is distributed in the copper matrix as a single substance in the copper, which can improve the debonding work of the metal copper ceramic interface, reduce the interface energy, and inhibit the segregation and growth of the alumina dispersed phase at the metal ceramic interface to improve the material performance.

[0026] Furthermore, the high-aluminum dispersed copper alloy material provided by the present invention can refine the grains after alloying with the added trace metal elements, thereby improving the material properties through grain refinement strengthening.

[0027] At the same time, the high-aluminum dispersed copper alloy material provided by the present invention also regulates the performance of the material by controlling the content of trace metal elements and aluminum oxide in the high-aluminum dispersed copper alloy material, thereby obtaining a high-aluminum dispersed copper alloy material with high hardness, high wear resistance, high conductivity and high elongation that meets the needs of broader market applications.

[0028] In addition, the present invention provides a method for preparing a high-aluminum dispersed copper alloy material, by adding a certain mass percentage of aluminum elements and trace metal elements with a lower reducibility than aluminum during the smelting process, so that the trace metal elements can be evenly distributed in the copper matrix, and then the aluminum and the copper alloy powder doped with trace metal elements with a lower reducibility than aluminum are evenly distributed by water atomization. Then, through the hot isostatic pressing process, sintering and internal oxidation are carried out simultaneously, and an aluminum oxide reinforcement phase is generated in situ, so that the aluminum oxide reinforcement phase and the copper matrix interface are well combined, and the metal elements with a lower reducibility than aluminum are evenly distributed in the high-aluminum dispersed copper alloy. At the same time, during the process of aluminum oxide generation, pressure is applied to break the aluminum oxide layer concentrated on the aluminum oxide surface in the copper alloy powder, prevent the aluminum oxide layer from deteriorating the sintering performance after the formation of the layer, and facilitate the discharge of gas in the copper alloy powder, which can greatly improve the density of the high-aluminum dispersed copper alloy ingot obtained by hot isostatic pressing. Finally, the excess oxygen source in the ingot is removed through hydrogen reduction, and then the ingot is densified by hot extrusion. At the same time, the grains are elongated, which can effectively avoid the problem of significant deterioration of the alloy's strength and plasticity caused by the formation of continuous or coarsely distributed alumina particles along the grain boundaries during high-temperature internal oxidation, thereby significantly improving the comprehensive performance of the alloy.

[0029] The invention provides a method for preparing a high-aluminum dispersed copper alloy material. The high-aluminum dispersed copper alloy material finally prepared has a density of ≥8.75g / cm 3, hardness ≥70HRB, conductivity ≥70%IACS, tensile strength ≥400MPa, elongation ≥10%, softening temperature ≥900℃, its performance can fully meet the needs of a wider market application. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A flow chart of a method for preparing a high-aluminum dispersed copper alloy material provided in an embodiment of the present invention.

[0031] Figure 2 A SEM photograph of a high-aluminum dispersed copper alloy material prepared by the method for preparing a high-aluminum dispersed copper alloy material provided in Example 1 of the present invention;

[0032] Figure 3 A SEM photograph of a high-aluminum dispersed copper alloy material prepared by the method for preparing a high-aluminum dispersed copper alloy material provided in Example 2 of the present invention;

[0033] Figure 4 A SEM photograph of a high-aluminum dispersed copper alloy material prepared by the method for preparing a high-aluminum dispersed copper alloy material provided in Example 3 of the present invention;

[0034] Figure 5 This is a SEM photo of a high-aluminum dispersed copper alloy material prepared by the preparation method of a high-aluminum dispersed copper alloy material provided in Comparative Example 1 of the present invention;

[0035] Figure 6 This is a SEM photograph of the high-aluminum dispersed copper alloy material prepared by the preparation method of the high-aluminum dispersed copper alloy material provided in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0036] The embodiment of the present invention provides a high-aluminum dispersed copper alloy material, which includes, by mass percentage, 0.4-2.0wt% of Al, 0.1-2.0wt% of a metal with a lower reducibility than aluminum, an oxygen content of <0.3wt%, and the remainder being Cu and unavoidable impurities.

[0037] Among them, the metal with lower reducing property than aluminum is one or more of Ti, Ag, Ni, Sn, Cr, Zr and Zn.

[0038] The present invention dopes a certain amount of aluminum into copper to form aluminum oxide dispersed copper, and at the same time dopes copper with a trace amount of metal elements whose reducibility is lower than that of aluminum. The trace metal elements are distributed in the copper matrix as a single substance in the copper, which can improve the debonding work at the metal copper ceramic interface, reduce the interface energy, and inhibit the segregation and growth of aluminum oxide dispersed phase at the metal ceramic interface to improve the material performance.

[0039] Furthermore, the trace metal elements added in the present invention can refine the grains after alloying, thereby improving the material properties through grain refinement strengthening.

[0040] At the same time, the present invention also regulates the performance of the material by controlling the content of trace metal elements and aluminum oxide in the high-aluminum dispersed copper alloy material, thereby obtaining a high-aluminum dispersed copper alloy material with high strength, hardness, high wear resistance, high conductivity and high elongation that meets the needs of broader market applications.

[0041] See also Figure 1 The present invention also provides a method for preparing a high-aluminum dispersed copper alloy material, comprising the following steps:

[0042] Step 1) Copper, aluminum and a metal with a lower reducing property than aluminum are mixed and smelted, and after smelting, a copper alloy powder containing 0.4-2.0wt% Al, 0.1-2.0wt% metal with a lower reducing property than aluminum, less than 0.3wt% oxygen, and the remainder Cu and unavoidable impurities is prepared by water atomization method.

[0043] The invention adds 0.4-2.0wt% of aluminum and 0.1-2.0wt% of trace metal elements with lower reducibility than aluminum during the smelting process, so that the aluminum and trace metal elements can be evenly distributed in the copper matrix, and then obtains the copper alloy powder in which the aluminum and the metal elements with lower reducibility than aluminum are evenly distributed through the water atomization method.

[0044] When copper, aluminum and metals with lower reducing power than aluminum are mixed and smelted, the smelting temperature is 1100° C.-1250° C. The particle size of the copper alloy powder obtained by the water atomization method is less than 60 meshes.

[0045] Wherein, the metal with lower reducing property than aluminum is one or more of Ti, Ag, Ni, Sn, Cr, Zr and Zn.

[0046] Step 2) The obtained copper alloy powder is mixed with an oxidant and then subjected to cold isostatic pressing to obtain a copper alloy blank.

[0047] The oxidant is Cu2O powder, and the particle size of the Cu2O powder is less than 500 meshes.

[0048] Among them, the cold isostatic pressing adopts a polyurethane mold, and the cold isostatic pressing pressure is 150-300MPa.

[0049] Step 3) The copper alloy blank is sealed with a sheath, and after evacuation, hot isostatic pressing is performed to obtain a high-aluminum dispersed copper alloy ingot.

[0050] The present invention subjects the copper alloy blank obtained by cold isostatic pressing to a hot isostatic pressing process, so that sintering and internal oxidation can be carried out simultaneously, and an aluminum oxide reinforcement phase is generated in situ, so that the aluminum oxide reinforcement phase and the copper matrix interface are well combined, and the doped metal element with a lower reducibility than aluminum is evenly distributed in the high-aluminum dispersed copper alloy. In addition, during the process of aluminum oxide generation, pressure is applied to break the aluminum oxide layer concentratedly precipitated on the aluminum oxide surface in the copper alloy powder, so as to prevent the sintering performance from being deteriorated after the aluminum oxide layer is formed, which is beneficial to the discharge of gas in the copper alloy powder, and can greatly improve the compactness of the high-aluminum dispersed copper alloy ingot obtained by hot isostatic pressing.

[0051] The temperature of the copper alloy blank after the vacuum is 500℃-600℃, the time is ≥10h, and the vacuum degree is less than 5×10 -3 Pa.

[0052] In addition, the hot isostatic pressing pressure is 30-200 MPa, the hot isostatic pressing temperature is 500° C.-1000° C., and the hot isostatic pressing time is 1-8 h.

[0053] Step 4) The high-aluminum dispersed copper alloy ingot is unwrapped and then reduced in a hydrogen atmosphere.

[0054] The invention can remove the excess oxygen source in the billet by reducing the high-aluminum dispersed copper alloy billet after the sheath is removed in a hydrogen atmosphere.

[0055] The reduction temperature in hydrogen atmosphere is 50-900° C., and the reduction time is 1-16 hours.

[0056] Step 5) hot-extrude the reduced high-aluminum dispersed copper alloy ingot to obtain a high-aluminum dispersed copper alloy material doped with trace elements.

[0057] The present invention performs hot extrusion on the high-aluminum dispersed copper alloy ingot, which can not only densify the high-aluminum dispersed copper alloy ingot, but also elongate the grains therein, and can effectively avoid the problem of significant deterioration of the strength and plasticity of the alloy caused by the formation of continuous or coarsely distributed aluminum oxide particles along the grain boundaries during high-temperature internal oxidation, thereby significantly improving the comprehensive performance of the alloy.

[0058] The hot extrusion temperature of the high aluminum dispersed copper alloy ingot is 700-950°C, and the extrusion ratio is 10-50.

[0059] The present invention provides a method for preparing a high-aluminum dispersed copper alloy material. The prepared high-aluminum dispersed copper alloy material can improve the electrical conductivity and elongation of the material while maintaining the hardness of the material, which is more conducive to subsequent processing and deformation treatment. The high-aluminum dispersed copper alloy material prepared by the present invention has a density of ≥8.75g / cm 3, hardness ≥70HRB, conductivity ≥70%IACS, tensile strength ≥400MPa, elongation ≥10%, softening temperature ≥900℃, its performance can fully meet the needs of a wider market application, and can be widely used in electrode materials, electrical contact materials, continuous casting machine crystallizers and other products.

[0060] The following is a detailed description of the preparation method of a high-aluminum dispersed copper alloy material provided by the present invention through examples.

[0061] Example 1

[0062] (1) Electrolytic copper, aluminum ingots, and titanium ingots are smelted at a temperature of 1150° C. in proportion to form a copper alloy melt having an Al content of 0.4% wt and a Ti content of 0.2% wt. After the melt is purified and impurities are removed, a copper-aluminum alloy powder is obtained by water atomization.

[0063] (2) After screening, alloy powder with a particle size less than 60 mesh and oxidant (Cu2O) were added to a V-type mixer and mixed for 4 hours.

[0064] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa and the pressure is maintained for 20 minutes. The green sheet density is 7.4 g / cm 3 .

[0065] (4) The pressed blank is sealed in an iron sleeve and vacuum-evacuated at 550°C for 10 h. It is then internally oxidized and sintered by hot isostatic pressing at 950°C and 150 MPa. After keeping the temperature for 5 h, the sleeve is removed and reduced in a hydrogen atmosphere to obtain a high-aluminum dispersed copper alloy ingot.

[0066] (5) The high aluminum dispersed copper alloy ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain a high aluminum dispersed copper alloy rod.

[0067] The high aluminum dispersed copper alloy rod prepared by the embodiment of the present invention is observed by scanning electron microscope. The obtained SEM photo is as follows: Figure 2 shown.

[0068] In addition, after testing, the density of the high aluminum dispersed copper alloy rod prepared in this embodiment is 8.83g / cm 3 , hardness 86.3HRB, conductivity 77.5%IACS, tensile strength 560MPa, elongation 15.7%.

[0069] Example 2

[0070] (1) Electrolytic copper, aluminum ingots, and titanium ingots are smelted at a temperature of 1150° C. in proportion to form a copper alloy melt having an Al content of 0.8% wt and a Ti content of 0.2% wt. After the melt is purified and impurities are removed, a copper-aluminum alloy powder is prepared by water atomization.

[0071] (2) After screening, alloy powder with a particle size less than 60 mesh and oxidant (Cu2O) were added to a V-type mixer and mixed for 4 hours.

[0072] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa and the pressure is maintained for 20 minutes. The green sheet density is 7.4 g / cm 3 .

[0073] (4) The pressed blank is sealed in an iron sleeve and vacuum-evacuated at 550°C for 10 h. It is then internally oxidized and sintered by hot isostatic pressing at 950°C and 150 MPa. After keeping the temperature for 5 h, the sleeve is removed and reduced in a hydrogen atmosphere to obtain a high-aluminum dispersed copper alloy ingot.

[0074] (5) The high aluminum dispersed copper alloy ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain a high aluminum dispersed copper alloy rod.

[0075] The high aluminum dispersed copper alloy rod prepared by the embodiment of the present invention is observed by scanning electron microscope. The obtained SEM photo is as follows: Figure 3 shown.

[0076] In addition, after testing, the density of the high aluminum dispersed copper alloy rod prepared in this embodiment is 8.83g / cm 3 , hardness 89.8HRB, conductivity 73.6%IACS, tensile strength 589MPa, elongation 10.5%.

[0077] Example 3

[0078] (1) Electrolytic copper, aluminum ingots, and silver ingots are smelted at a temperature of 1150° C. in proportion to form a copper alloy melt having an Al content of 0.4% wt and an Ag content of 0.2% wt. After the melt is purified and impurities are removed, a copper-aluminum alloy powder is prepared by water atomization.

[0079] (2) After screening, alloy powder with a particle size less than 60 mesh and oxidant (Cu2O) were added to a V-type mixer and mixed for 4 hours.

[0080] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa and the pressure is maintained for 20 minutes. The green sheet density is 7.4 g / cm 3 .

[0081] (4) The pressed blank is sealed in an iron sleeve and vacuum-evacuated at 550°C for 10 h. It is then internally oxidized and sintered by hot isostatic pressing at 950°C and 150 MPa. After keeping the temperature for 5 h, the sleeve is removed and reduced in a hydrogen atmosphere to obtain a high-aluminum dispersed copper alloy ingot.

[0082] (5) The high aluminum dispersed copper alloy ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain a high aluminum dispersed copper alloy rod.

[0083] The high aluminum dispersed copper alloy rod prepared by the embodiment of the present invention is observed by scanning electron microscope. The obtained SEM photo is as follows: Figure 4 shown.

[0084] In addition, after testing, the density of the high aluminum dispersed copper alloy rod prepared in this embodiment is 8.83g / cm 3 , hardness 84.3HRB, conductivity 80.4%IACS, tensile strength 524MPa, elongation 18.0%.

[0085] Comparative Example 1

[0086] (1) Electrolytic copper and aluminum ingots are smelted in proportion at a temperature of 1150° C. to form a copper-aluminum alloy melt with an Al content of 0.8% wt. After the melt is purified and impurities are removed, a copper-aluminum alloy powder is prepared by water atomization.

[0087] (2) After screening, alloy powder with a particle size less than 60 mesh and oxidant (Cu2O) were added to a V-type mixer and mixed for 4 hours.

[0088] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa and the pressure is maintained for 20 minutes. The green sheet density is 7.4 g / cm 3 .

[0089] (4) The pressed blank is sealed in an iron sleeve and vacuum-evacuated at 550°C for 10 h. It is then internally oxidized and sintered by hot isostatic pressing at 950°C and 150 MPa. After keeping the temperature for 5 h, the sleeve is removed and reduced in a hydrogen atmosphere to obtain a high-aluminum dispersed copper alloy ingot.

[0090] (5) The high aluminum dispersed copper alloy ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain a high aluminum dispersed copper alloy rod.

[0091] The high aluminum dispersed copper alloy rod prepared in this comparative example was observed by scanning electron microscope. The obtained SEM photo is as follows Figure 5 shown.

[0092] In addition, after testing, the density of the high aluminum dispersed copper alloy rod prepared in this comparative example is 8.82g / cm3 , hardness 79.2HRB, conductivity 68.7%IACS, tensile strength 467MPa, elongation 6.2%.

[0093] Comparative Example 2

[0094] (1) Electrolytic copper and aluminum ingots are smelted in proportion at a temperature of 1150° C. to form a copper-aluminum alloy melt with an Al content of 0.4%wt. After the melt is purified and impurities are removed, a copper-aluminum alloy powder is prepared by water atomization.

[0095] (2) After screening, alloy powder with a particle size less than 60 mesh and oxidant (Cu2O) were added to a V-type mixer and mixed for 4 hours.

[0096] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa and the pressure is maintained for 20 minutes. The green sheet density is 7.4 g / cm 3 .

[0097] (4) The pressed blank is sealed in an iron sleeve and vacuum-evacuated at 550°C for 10 h. It is then internally oxidized and sintered by hot isostatic pressing at 950°C and 150 MPa. After keeping the temperature for 5 h, the sleeve is removed and reduced in a hydrogen atmosphere to obtain a high-aluminum dispersed copper alloy ingot.

[0098] (5) The high aluminum dispersed copper alloy ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain a high aluminum dispersed copper alloy rod.

[0099] The high aluminum dispersed copper alloy rod prepared in this comparative example was observed by scanning electron microscope. The obtained SEM photo is as follows Figure 6 shown.

[0100] In addition, after testing, the density of the high aluminum dispersed copper alloy rod prepared in this comparative example is 8.82g / cm 3 , hardness 81.7HRB, conductivity 81.0%IACS, tensile strength 485MPa, elongation 13.0%.

[0101] From the comparison of SEM photos of the high-aluminum dispersed copper alloy materials obtained by Examples 1-3 of the present invention and Comparative Examples 1-2 and the comparison of the performance of the high-aluminum dispersed copper alloy materials obtained by Examples 1-3 of the present invention and Comparative Examples 1-2, it can be seen that when the aluminum content is low, such as Comparative Example 2, when the copper alloy rod is prepared with an aluminum content of 0.4%, the performance of the copper alloy rod meets the requirements without doping trace elements, but from the microscopic morphology, the distribution of aluminum oxide is relatively dispersed. After doping a certain amount of trace elements in Examples 1 and 3 of the present invention, the hardness of the sample can be greatly improved under the condition of a slight decrease in conductivity and elongation, and from the microscopic morphology, the better dispersion distribution of aluminum oxide is not affected. When the aluminum content is high, such as Comparative Example 1, when the copper alloy rod is prepared with an aluminum content of 0.8%, the performance of the copper alloy rod prepared is poor, and from the microscopic morphology, an aluminum oxide layer appears, and the aluminum oxide distribution is uneven. After a certain amount of Ag element is doped in Example 2 of the present invention, it can be seen that the aluminum oxide particles are dispersed more evenly, and the hardness, conductivity, elongation and other properties are greatly improved.

[0102] Therefore, the preparation method of a high-aluminum dispersed copper alloy material provided in an embodiment of the present invention can improve the conductivity and elongation of the material while maintaining the hardness of the obtained high-aluminum dispersed copper alloy material by adding a certain mass percentage of trace metal elements with a lower reducibility than aluminum into the high-aluminum dispersed copper alloy, which is more conducive to subsequent processing and deformation treatment, thereby expanding the application scenarios of the dispersion-strengthened copper alloy material.

[0103] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A high aluminum dispersed copper alloy material, characterized in that: Calculated by mass percentage, it includes 0.4-2.0wt% of Al, 0.1-2.0wt% of metal with lower reducibility than aluminum, oxygen content <0.3wt%, and the balance is Cu and unavoidable impurities.

2. The high aluminum dispersed copper alloy material according to claim 1, characterized in that: The metal having a lower reducing property than aluminum is one or more of Ti, Ag, Ni, Sn, Cr, Zr and Zn.

3. A method for preparing a high-aluminum dispersed copper alloy material, characterized in that: The steps include: Copper, aluminum and a metal with a lower reducing power than aluminum are mixed and smelted, and after smelting, a copper alloy powder containing 0.4-2.0wt% of Al, 0.1-2.0wt% of a metal with a lower reducing power than aluminum, less than 0.3wt% of oxygen, and the remainder being Cu and unavoidable impurities is prepared by water atomization method; The copper alloy powder is mixed with an oxidant and then cold isostatically pressed to obtain a copper alloy blank; The copper alloy blank is sealed by encapsulation, and then hot isostatically pressed to obtain a high-aluminum dispersed copper alloy ingot after vacuuming. The high aluminum dispersed copper alloy ingot is unwrapped and reduced in a hydrogen atmosphere; hot-extrude the reduced high-aluminum dispersed copper alloy ingot to obtain a high-aluminum dispersed copper alloy material doped with trace elements; Wherein, the metal with lower reducing property than aluminum is one or more of Ti, Ag, Ni, Sn, Cr, Zr and Zn.

4. The method for preparing a high aluminum dispersed copper alloy material according to claim 3, characterized in that: The smelting temperature during smelting is 1100° C.-1250° C., and the particle size of the copper alloy powder is less than 60 meshes.

5. The method for preparing a high aluminum dispersed copper alloy material according to claim 3, characterized in that: The oxidant is Cu2O powder, and the particle size of the Cu2O powder is less than 500 meshes.

6. The method for preparing a high aluminum dispersed copper alloy material according to claim 3, characterized in that: The cold isostatic pressing adopts a polyurethane mold, and the cold isostatic pressing pressure is 150-300MPa.

7. The method for preparing a high aluminum dispersed copper alloy material according to claim 3, characterized in that: The temperature of the copper alloy blank after the encapsulation is 500°C-600°C, the time is ≥10h, and the vacuum degree is less than 5×10 -3 Pa.

8. The method for preparing a high aluminum dispersed copper alloy material according to claim 7, characterized in that: The hot isostatic pressing pressure is 30-200 MPa, the hot isostatic pressing temperature is 500° C.-1000° C., and the hot isostatic pressing time is 1-8 hours.

9. The method for preparing a high aluminum dispersed copper alloy material according to claim 3, characterized in that: The reduction temperature in the hydrogen atmosphere is 50-900° C., and the reduction time is 1-16 hours.

10. The method for preparing a high aluminum dispersed copper alloy material according to claim 3, characterized in that: The extrusion temperature during the hot extrusion is 700-950° C., and the extrusion ratio is 10-50.