Aluminum oxide dispersion strengthened copper-based composite material bar and preparation method thereof

A method for preparing alumina dispersion strengthened copper-based composite materials addresses the challenges of high-aluminum content by ensuring uniform distribution of trace metals and alumina reinforcement, enhancing material properties for improved spot welding performance.

CN119061287APending Publication Date: 2024-12-03ZHUZHOU SMELTER GRP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410972389.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing alumina dispersion strengthened copper-based composite materials face challenges in high-aluminum content due to reverse diffusion and formation of continuous internal oxide films, leading to incomplete oxidation and impaired hardness, conductivity, and other properties, limiting their application in demanding scenarios like spot welding.

Method used

A method involving smelting copper, aluminum, and a metal with lower reducing properties, followed by water atomization, cold isostatic pressing, vacuum hot isostatic pressing, reduction, and hot extrusion to create a composite material with evenly distributed trace metal elements, promoting alumina reinforcement phase generation and breaking surface alumina layers, enhancing material properties.

Benefits of technology

The method results in a composite material with improved hardness, conductivity, and elongation, suitable for spot welding applications, by preventing alumina particle segregation and maintaining material integrity through fine grain strengthening and uniform distribution of trace metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061287A_ABST
    Figure CN119061287A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum oxide dispersion strengthened copper-based composite material bar and a preparation method thereof, and belongs to the field of metal-based composite materials. According to the method, trace metal elements with the reducibility lower than that of aluminum are added in the smelting process, the trace metal elements can be evenly distributed in a matrix in the form of simple substances, and then the alloy powder with the evenly-distributed aluminum and trace metal elements is obtained through a water atomization method. Then sintering and internal oxidation are synchronously carried out through a hot isostatic pressing process, an aluminum oxide reinforced phase is generated in situ, meanwhile, pressurization is carried out in the aluminum oxide generation process, sintering performance deterioration caused after an aluminum oxide layer is formed is prevented, gas exhaust is facilitated, and compactness is improved. And after excessive oxygen sources in the billets are removed through hydrogen reduction subsequently, the billets are densified in a hot extrusion mode, meanwhile, crystal grains are lengthened, and the comprehensive performance of the bar is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal matrix composite materials, and in particular to an alumina dispersion strengthened copper matrix composite material rod and a preparation method thereof. Background Art

[0002] Alumina dispersion strengthened copper-based composite materials have excellent high-temperature properties such as high strength, high hardness, high conductivity and high softening temperature, and have broad market application prospects in rail transportation, aerospace, automobile and other fields. Many researchers at home and abroad have actively explored the preparation process of high-performance alumina dispersion strengthened copper-based composite materials to obtain dispersion strengthened copper-based composite materials with excellent performance. In Europe and the United States, alumina dispersion strengthened copper-based composite materials prepared by internal oxidation method have now formed an electrode material industry chain. Among them, the alumina dispersion strengthened copper-based composite materials of grades such as C15715, C15740 and C15760 produced by SCM Company in the United States by internal oxidation method have a daily production scale of 20t. There are also domestic enterprises such as Guangzhou Nonferrous Metals, China Aluminum Luotong, and China Shipbuilding Industry Corporation that produce alumina dispersion strengthened copper-based composite materials, and their products are all concentrated in low-aluminum dispersion strengthened copper-based composite materials.

[0003] However, the welding of materials such as new energy batteries, aluminum alloys, high-strength steel, galvanized plates, and nickel-plated plates requires high quality spot welding, and the spot welding itself is difficult. In addition, other application scenarios have higher requirements for the hardness, strength, wear resistance and other properties of the material. Therefore, high-aluminum dispersion-strengthened copper-based composite materials with better performance are needed. Generally, the reverse diffusion trend of Al increases during the internal oxidation of high-aluminum dispersion-strengthened copper-based composite materials, resulting in the formation of a continuous internal oxide film inside the material, which hinders the further occurrence of internal oxidation and causes incomplete internal oxidation; in addition, due to the high concentration of solute elements, A12O3 particles are easy to grow during the internal oxidation process, which inhibits the strengthening effect and affects the hardness, conductivity and other properties of the material, which limits the application of high-aluminum dispersion-strengthened copper-based composite materials. Summary of the invention

[0004] In order to improve the performance of an alumina dispersion strengthened copper-based composite material, an embodiment of the present application provides an alumina dispersion strengthened copper-based composite material rod and a preparation method thereof.

[0005] A first aspect of the present invention provides a method for preparing an alumina dispersion strengthened copper-based composite material rod, comprising:

[0006] The copper, aluminum and a metal with a lower reducing property than aluminum are smelted, and alloy powder is prepared by water atomization; the alloy powder comprises the following components by mass percentage: 0.1-2.0% aluminum, 0.1-2.0% metal with a lower reducing property than aluminum, less than 0.3% oxygen content, and the balance is copper;

[0007] The alloy powder is mixed with an oxidant and then cold isostatically pressed to obtain a preform;

[0008] The raw blank is sealed in a bag, vacuum-evacuated, and hot isostatically pressed to obtain an alumina dispersion-strengthened copper-based composite material ingot;

[0009] Unwrapping the alumina dispersion strengthened copper-based composite material ingot and then reducing it;

[0010] The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded to prepare alumina dispersion strengthened copper-based composite material rods.

[0011] In some embodiments, the metal having a lower reducing property than aluminum includes Ti, Ag, Ni, Sn, Cr, Zr, or Zn.

[0012] In some embodiments, the smelting temperature is 1100°C-1250°C.

[0013] In some embodiments, the alloy powder has a particle size of less than 60 mesh, the oxidant is Cu2O powder, and the powder particle size of the oxidant is less than 500 mesh.

[0014] In some embodiments, the cold isostatic pressing pressure is 150-300 MPa, and the holding time is 10-30 min.

[0015] In some embodiments, the temperature of the vacuum pumping is 500°C-600°C, and the vacuum degree of the vacuum pumping is less than 5*10 -3 Pa, the vacuum pumping time is ≥10h.

[0016] In some embodiments, the temperature of the hot isostatic pressing is 500° C.-1000° C., the pressure of the hot isostatic pressing is 30-200 MPa, and the time of the hot isostatic pressing is 1-8 h.

[0017] In some embodiments, the reducing atmosphere is hydrogen, the reducing temperature is 50-900° C., and the reducing time is 1-16 hours.

[0018] In some embodiments, the hot extrusion temperature is 700-950° C., and the extrusion ratio is 10-50.

[0019] The second aspect of the present invention provides an alumina dispersion strengthened copper-based composite material rod, comprising the following components by mass percentage: 0.1-2.0% alumina, 0.1-2.0% metal with a lower reducing property than aluminum, and the rest copper.

[0020] The present invention provides an alumina dispersion-strengthened copper-based composite material bar and a preparation method thereof. In the method, a trace metal element with a lower reducibility than aluminum is added during the smelting process, so that the trace metal element can be evenly distributed in the matrix as a single substance, and then an alloy powder with uniform distribution of aluminum and trace metal elements is obtained by a water atomization method. Then, a hot isostatic pressing process is used to synchronize sintering and internal oxidation, and an alumina reinforcement phase is generated in situ, so that the interface of the alumina reinforcement phase and the copper matrix is ​​well bonded, and the trace metal elements are evenly distributed. At the same time, pressure is applied during the generation of alumina, so that the alumina layer concentrated on the powder surface is broken, and the sintering performance is prevented from being deteriorated after the formation of the alumina layer, which is conducive to exhausting gas and improving density. Subsequently, the billet is further densified by hot extrusion after the excess oxygen source in the billet is removed by hydrogen reduction, and the grains are elongated at the same time, effectively avoiding the significant deterioration of the alloy strength and plasticity caused by the continuous or coarse distribution of alumina particles along the grain boundaries during the high-temperature internal oxidation process, and significantly improving the comprehensive performance of the alumina dispersion-strengthened copper-based composite material bar. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A flowchart of a method for preparing an alumina dispersion strengthened copper-based composite material rod provided according to some embodiments is exemplified;

[0022] Figure 2 This is a SEM electron microscope image of the rod prepared in Example 1 of the examples of the present application;

[0023] Figure 3 This is a SEM electron microscope image of the rod prepared in Example 2 of the examples of the present application;

[0024] Figure 4 This is a SEM electron microscope image of the rod prepared in Example 3 of the examples of the present application;

[0025] Figure 5 This is a SEM electron microscope image of the rod prepared in Example 4 of the present application;

[0026] Figure 6 This is a SEM electron microscope image of the rod prepared in Example 5 of the present application;

[0027] Figure 7 This is a SEM electron microscope image of the rod prepared in Comparative Example 1 in the examples of the present application;

[0028] Figure 8 This is a schematic diagram of cracking and water leakage in the electrode cap during welding;

[0029] Fig. 9 This is a SEM electron microscope image of the rod prepared in Comparative Example 2 in the examples of the present application;

[0030] Fig.10 This is a SEM electron microscope image of the rod prepared in Comparative Example 3 in the examples of the present application. DETAILED DESCRIPTION

[0031] In order to better understand the above technical solution, the technical solution of the present application is described in detail below through specific implementation methods.

[0032] The present application provides a method for preparing an alumina dispersion strengthened copper-based composite material rod. Figure 1 The flowchart of a method for preparing an alumina dispersion strengthened copper-based composite rod according to some embodiments is exemplarily shown. The method includes S100-S500.

[0033] S100, smelting electrolytic copper, aluminum and a metal with a lower reducing property than aluminum, and preparing alloy powder by water atomization; the alloy powder comprises the following components by mass percentage: 0.1-2.0% aluminum, 0.1-2.0% metal with a lower reducing property than aluminum, less than 0.3% oxygen content, and the balance copper.

[0034] In this technical solution, if the Al content exceeds 2%, the strengthening phase cannot be dispersed, and if it is less than 0.1%, the strengthening effect is insufficient and the hardness is very low, so the mass percentage of aluminum is set to 0.1-2.0%.

[0035] In the embodiments of the present application, trace metal elements with a lower reducing power than aluminum are added during the smelting process. The trace metal elements do not combine with oxygen to form oxides, but are evenly distributed in the matrix as a single substance. Then, an alloy powder with evenly distributed aluminum and trace metal elements is obtained by water atomization.

[0036] The oxygen content in the alloy powder can be controlled by controlling the nozzle angle and water pressure of the water atomization equipment.

[0037] In the embodiment of the present application, the copper to be smelted may be electrolytic copper, and the aluminum may be aluminum ingots. Metals with a lower reducibility than aluminum may be used in the form of blocks, for example, when the metal with a lower reducibility than aluminum is Ti, titanium blocks may be used.

[0038] In some embodiments, the metal having a lower reducing property than aluminum includes Ti, Ag, Ni, Sn, Cr, Zr, or Zn.

[0039] In some embodiments, copper, aluminum and metals with lower reducing properties than aluminum are smelted in a medium frequency furnace at a smelting temperature of 1100°C-1250°C.

[0040] In this technical solution, if the melting temperature is too high, it will cause burns, and if it is too low, it will affect the melting effect and the alloy will have segregation problems, so the capacity temperature is set to 1100℃-1250℃.

[0041] In some embodiments, copper, aluminum and a metal with a lower reducing property than aluminum are smelted to obtain a melt, and after purifying and removing impurities from the melt, alloy powder is prepared by water atomization.

[0042] S200, mixing the alloy powder and the oxidant, and then performing cold isostatic pressing to obtain a green blank.

[0043] In some embodiments, the alloy powder has a particle size of less than 60 mesh, the oxidant is Cu2O powder, and the oxidant has a powder particle size of less than 500 mesh. The alloy powder with a particle size of less than 60 mesh and the Cu2O powder with a powder particle size of less than 500 mesh are added to a V-type mixer for mixing, and the mixing time is greater than or equal to 4 hours.

[0044] In this technical solution, alloy powders larger than 60 mesh are used to prepare rods, and their performance is poor. If the cuprous oxide powder is finer, the oxygen source can be better dispersed, allowing more sites for the in-situ grown alumina dispersed phase to form and better distribution. If the mixing time is less than 4 hours, the alloy powder and cuprous oxide powder cannot be mixed evenly, and segregation will occur.

[0045] In some embodiments, the cold isostatic pressing pressure is 150-300 MPa, and the holding time is 10-30 min. In some embodiments, the polyurethane mold has a diameter of ≥260 mm and a length of ≥1200 mm.

[0046] In the embodiment of the present application, a polyurethane mold can be used for cold isostatic pressing.

[0047] S300, sealing the preliminary blank in a package, vacuuming and hot isostatic pressing to obtain an alumina dispersion strengthened copper-based composite material ingot.

[0048] In the embodiment of the present application, sintering and internal oxidation are carried out simultaneously through the hot isostatic pressing process, and the alumina reinforcement phase is generated in situ, so that the interface between the alumina reinforcement phase and the copper matrix is ​​better bonded, and the trace metal elements are evenly distributed. At the same time, pressure is applied during the alumina generation process to break up the alumina layer concentrated on the powder surface, preventing the sintering performance from deteriorating after the alumina layer is formed, which is beneficial to the discharge of gas and improves the density.

[0049] In some embodiments, the temperature of the vacuum pumping is 500°C-600°C, and the vacuum degree of the vacuum pumping is less than 5*10 -3 Pa, the vacuum pumping time is ≥10h.

[0050] In some embodiments, the hot isostatic pressing temperature is 500°C-1000°C, the hot isostatic pressing pressure is 30-200MPa, the hot isostatic pressing time is 1-8h, and the alumina dispersion strengthened copper-based composite material ingot obtained after hot isostatic pressing is a densified alumina dispersion strengthened copper-based composite material ingot.

[0051] In this technical solution, if the hot isostatic pressing temperature is too low and the time is too short, the sintering will be incomplete, and if the temperature is too high and the time is too long, the copper matrix grains will be coarse, reducing the fine grain strengthening effect, so the hot isostatic pressing temperature is set to 500℃-1000℃.

[0052] S400, unpacking the alumina dispersion strengthened copper-based composite material ingot and then reducing it.

[0053] In some embodiments, the reducing atmosphere is hydrogen, the reducing temperature is 50-900° C., and the reducing time is 1-16 hours.

[0054] S500, preparing an alumina dispersion strengthened copper-based composite material rod by hot extruding the reduced alumina dispersion strengthened copper-based composite material ingot.

[0055] In some embodiments, the hot extrusion temperature is 700-950° C., and the extrusion ratio is 10-50.

[0056] In this technical solution, if the extrusion temperature is too high, exceeding 950°C, peeling and cracking will occur on the surface of the rod after extrusion. If it is lower than 700°C, the dispersed copper ingot cannot be extruded.

[0057] In the embodiments of the present application, after removing the excess oxygen source in the ingot through hydrogen reduction, the ingot is further densified by hot extrusion, while the grains are elongated, thereby effectively avoiding the significant deterioration of the strength and plasticity of the alloy caused by the formation of continuous or coarsely distributed alumina particles along the grain boundaries during the high-temperature internal oxidation process, and significantly improving the comprehensive performance of the alumina dispersion-strengthened copper-based composite material rods.

[0058] The preparation method of the embodiment of the present application is reasonable and easy to operate. It can improve the performance of high-aluminum dispersion-strengthened copper-based composite materials by adding trace metal elements while adding an aluminum oxide phase. It can also improve the conductivity and elongation of the material while maintaining the hardness of the material, which is more conducive to post-processing deformation treatment. It can be applied to spot welding electrode materials to improve their welding performance.

[0059] The present application also provides an alumina dispersion strengthened copper-based composite material rod, which includes the following components in mass percentage: 0.1-2.0% alumina, 0.1-2.0% metal with a lower reducing property than aluminum, and the rest copper.

[0060] In some embodiments, the performance of the alumina dispersion strengthened copper-based composite rod can be controlled by adjusting the content of the metal with a lower reducibility than aluminum and the alumina dispersed phase.

[0061] In the embodiment of the present application, alumina dispersion-strengthened copper-based composite material rods are doped with trace metal elements with a lower reducibility than aluminum, and the trace metal elements are distributed in the matrix as a single substance in the dispersion-strengthened copper-based composite material, and the material properties are improved by increasing the debonding work of the metal-ceramic interface (i.e., the interface between copper and alumina), reducing the interface energy, and inhibiting the segregation and growth of the alumina dispersed phase at the metal-ceramic interface. At the same time, adding alloying elements can refine the grains, and improve the material properties through fine grain strengthening. At the same time, the product performance can be regulated by controlling the content of trace metal elements and alumina, and an alumina dispersion-strengthened copper-based composite material rod with high hardness, high wear resistance, high conductivity and high elongation that meets market demand is prepared.

[0062] In some embodiments, the density of the alumina dispersion strengthened copper-based composite rod is ≥8.75 g / cm 3 , hardness ≥70HRB, conductivity ≥70%IACS, tensile strength ≥400MPa, elongation ≥10%, softening temperature ≥900℃.

[0063] Example 1 A method for preparing alumina dispersion-strengthened copper-based composite material rod

[0064] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted at a temperature of 1150° C. in proportion to form a melt. After the melt is purified and impurities are removed, alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.8%wt, Ti 0.8%wt, oxygen content 0.03%wt, and the rest is copper;

[0065] (2) After screening, alloy powder with a particle size less than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0066] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0067] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10 -3 After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0068] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0069] After testing, the density of the alumina dispersion strengthened copper-based composite rod prepared in this embodiment is 8.83 g / cm 3 , hardness 90.35HRB, conductivity 70.5%IACS, tensile strength 609MPa, elongation 12%, after 9000 spot welding points, the remaining length of the electrode cap is 21.69mm. Figure 2 This is a SEM electron microscope image of the rod prepared in Example 1 of the examples of the present application.

[0070] Example 2 A method for preparing alumina dispersion strengthened copper-based composite material rod

[0071] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted at a temperature of 1150° C. in proportion to form a melt. After the melt is purified and impurities are removed, alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.8%wt, Ag 0.1%wt, oxygen content of 0.031%wt, and the rest is copper;

[0072] (2) After screening, alloy powder with a particle size less than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0073] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0074] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10 -3 After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0075] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0076] After testing, the density of the alumina dispersion strengthened copper-based composite rod prepared in this embodiment is 8.83 g / cm 3, hardness 82.6HRB, conductivity 73.1%IACS, tensile strength 584MPa, elongation 11.2%, after 9000 spot welding points, the remaining length of the electrode cap is 19.65mm. Figure 3 This is a SEM electron microscope image of the rod prepared in Example 2 of the examples of this application.

[0077] Example 3 A method for preparing alumina dispersion strengthened copper-based composite material rod

[0078] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted at a temperature of 1150° C. in proportion to form a melt. After the melt is purified and impurities are removed, alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.4%wt, Ag 0.2%wt, oxygen content of 0.026%wt, and the rest is copper;

[0079] (2) After screening, alloy powder with a particle size less than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0080] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0081] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10 -3 After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0082] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0083] After testing, the density of the alumina dispersion strengthened copper-based composite rod prepared in this embodiment is 8.83 g / cm 3 , hardness 84.3HRB, conductivity 80.4%IACS, tensile strength 524MPa, elongation 18.0%, after 9000 spot welding points, the remaining length of the electrode cap is 20.05mm. Figure 4 This is a SEM electron microscope image of the rod prepared in Example 3 of the examples of the present application.

[0084] Example 4 A method for preparing alumina dispersion strengthened copper-based composite material rod

[0085] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted at a temperature of 1150° C. in proportion to form a melt. After the melt is purified and impurities are removed, alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.8%wt, Ti 0.2%wt, oxygen content of 0.036%wt, and the rest is copper;

[0086] (2) After screening, alloy powder with a particle size less than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0087] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0088] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10 -3 After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0089] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0090] After testing, the density of the alumina dispersion strengthened copper-based composite rod prepared in this embodiment is 8.83 g / cm 3 , hardness 89.8HRB, conductivity 73.6%IACS, tensile strength 589MPa, elongation 10.5%, after 9000 spot welding points, the remaining length of the electrode cap is 21.02mm. Figure 5 This is a SEM electron microscope image of the rod prepared in Example 4 of the examples of the present application.

[0091] Example 5 A method for preparing alumina dispersion strengthened copper-based composite material rod

[0092] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted in proportion at a temperature of 1150° C. to form a melt, and after the melt is purified and impurities are removed, an alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.4%wt, Ti 0.2%wt, oxygen content of 0.036%wt, and the rest is copper;

[0093] (2) After screening, alloy powder with a particle size less than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0094] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0095] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10 -3 After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0096] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0097] After testing, the density of the alumina dispersion strengthened copper-based composite rod prepared in this embodiment is 8.83 g / cm 3 , hardness 86.3HRB, conductivity 77.5%IACS, tensile strength 560MPa, elongation 15.7%, after 9000 spot welding points, the remaining length of the electrode cap is 20.27mm. Figure 6 This is a SEM electron microscope image of the rod prepared in Example 5 of the examples of the present application.

[0098] Comparative Example 1

[0099] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted at a temperature of 1150° C. in proportion to form a melt. After the melt is purified and impurities are removed, an alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.8%wt, oxygen content 0.029%wt, and the rest is copper;

[0100] (2) After screening, alloy powder with a particle size less than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0101] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0102] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10 -3After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0103] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0104] After testing, the density of the alumina dispersion strengthened copper-based composite rod prepared in this embodiment is 8.82 g / cm 3 , hardness 79.2HRB, conductivity 68.7%IACS, tensile strength 467MPa, elongation 6.2%, after 9000 spot welding points, the remaining length of the electrode cap is 18.16mm, and the electrode cap cracks and leaks during the welding process. Figure 7 This is a SEM electron microscope image of the rod prepared in Comparative Example 1 in the examples of the present application. Figure 8 This is a schematic diagram of cracking and leakage of the electrode cap during welding.

[0105] Comparing Comparative Example 1 with Example 1, it can be seen that when the aluminum content reaches 0.8%wt, the performance of the sample prepared by the current preparation process is poor, an aluminum oxide layer appears, and the dispersed phase cannot be dispersed. However, after doping with a trace amount of Ag element, it can be seen that the aluminum oxide particles are dispersed more evenly, and the hardness, conductivity, elongation and other properties are greatly improved. At the same time, the remaining length after welding is also longer, which increases the life of the electrode cap.

[0106] Comparative Example 2

[0107] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted at a temperature of 1150° C. in proportion to form a melt. After the melt is purified and impurities are removed, alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.4%wt, oxygen content 0.035%wt, and the rest is copper;

[0108] (2) After screening, alloy powder with a particle size less than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0109] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0110] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10-3 After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0111] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0112] After testing, the density of the alumina dispersion strengthened copper-based composite material prepared in this embodiment is 8.82 g / cm 3 , hardness 81.7HRB, conductivity 81.0%IACS, tensile strength 485MPa, elongation 13.0%, after 9000 spot welding points, the remaining length of the electrode cap is 18.96mm. Fig. 9 This is a SEM electron microscope image of the rod prepared in Comparative Example 2 in the examples of the present application.

[0113] Comparing Comparative Example 2 with Example 3, it can be seen that both samples are prepared with a moderate aluminum content of 0.4%. The performance of the samples is good without doping with trace elements. However, after doping with a certain amount of trace elements, the hardness of the samples can be improved while the conductivity and elongation are slightly reduced. At this time, the service life of the electrode cap can be increased. It can also be seen from the remaining length after welding that the remaining length of the doped samples is longer.

[0114] Comparative Example 3

[0115] (1) electrolytic copper, aluminum ingots, and titanium blocks are smelted at a temperature of 1150° C. in proportion to form a melt. After the melt is purified and impurities are removed, alloy powder is prepared by water atomization. The alloy powder includes the following components in terms of mass percentage: Al 0.4%wt, oxygen content 0.035%wt, and the rest is copper;

[0116] (2) After screening, alloy powder with a particle size greater than 60 mesh and an oxidant (Cu2O) are added to a V-type mixer and mixed for 4 hours;

[0117] (3) The mixed powder is placed in a polyurethane mold and cold isostatically pressed to obtain a green sheet. The cold isostatic pressing pressure is 200 MPa, the holding time is 20 min, and the green sheet density is 7.4 g / cm 3 ;

[0118] (4) The pressed blank is placed in an iron sleeve and sealed, and vacuumed for 10 hours at a temperature of 550°C to achieve a vacuum degree of 1.2*10 -3After Pa, internal oxidation sintering is carried out by hot isostatic pressing at a temperature of 950°C and a pressure of 150MPa. The hot isostatic pressing time is 5h, that is, after keeping warm for 5h, the sheath is unpacked and reduced in a hydrogen atmosphere to obtain a reduced alumina dispersion strengthened copper-based composite material ingot.

[0119] (5) The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded at 900° C. with an extrusion ratio of 36 to obtain an alumina dispersion strengthened copper-based composite material rod.

[0120] After testing, the density of the alumina dispersion strengthened copper-based composite rod prepared in this embodiment is 8.82 g / cm 3 , hardness 79.5HRB, conductivity 77.3%IACS, tensile strength 423MPa, elongation 11.0%. Fig.10 This is a SEM electron microscope image of the rod prepared in Comparative Example 3 in the examples of the present application.

[0121] Comparing Comparative Example 3 with Comparative Example 1, when the particle size of the alloy powder is too large, the overall performance of the rod will be reduced.

[0122] In summary, the aluminum oxide dispersion strengthened copper-based composite rod and its preparation method provided by the present invention, in which a trace metal element with a lower reducibility than aluminum is used for doping in the aluminum oxide dispersion strengthened copper-based composite material, the trace metal element is distributed in the matrix as a single substance in the dispersion strengthened copper-based composite material, and the material performance is improved by increasing the metal-ceramic interface debonding work, reducing the interface energy, and inhibiting the segregation and growth of the aluminum oxide dispersed phase at the metal-ceramic interface. At the same time, adding alloying elements can refine the grains, and improve the material performance through fine grain strengthening. At the same time, the product performance can be regulated by controlling the content of trace metal elements and aluminum oxide, and a dispersion strengthened copper-based composite product with high hardness, high wear resistance, high conductivity and high elongation that meets market demand can be prepared. By adding trace metal elements during the smelting process, the trace metal elements can be evenly distributed in the matrix, and then the alloy powder with aluminum and doping elements evenly distributed is obtained by water atomization. Then, the hot isostatic pressing process is used to synchronize sintering and internal oxidation, and an alumina reinforcement phase is generated in situ, so that the interface between the alumina reinforcement phase and the copper matrix is ​​well bonded, and the doping elements are evenly distributed. At the same time, pressure is applied during the alumina generation process to break the alumina layer concentrated on the powder surface, preventing the sintering performance from deteriorating after the alumina layer is formed, which is conducive to exhausting gas and improving density. Subsequently, the excess oxygen source in the billet is removed by hydrogen reduction, and then the billet is further densified by hot extrusion, while the grains are elongated, effectively avoiding the significant deterioration of the strength and plasticity of the alloy caused by the formation of continuous or coarsely distributed alumina particles along the grain boundaries during high-temperature internal oxidation, and significantly improving the comprehensive performance of the alloy.

[0123] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed. The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementation methods of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. A method for preparing an alumina dispersion strengthened copper-based composite rod, It is characterized in that include: The copper, aluminum and a metal with a lower reducing property than aluminum are smelted, and alloy powder is prepared by water atomization; the alloy powder comprises the following components by mass percentage: 0.1-2.0% aluminum, 0.1-2.0% metal with a lower reducing property than aluminum, less than 0.3% oxygen content, and the balance is copper; The alloy powder is mixed with an oxidant and then cold isostatically pressed to obtain a preform; The raw blank is sealed in a bag, vacuum-evacuated, and hot isostatically pressed to obtain an alumina dispersion-strengthened copper-based composite material ingot; Unwrapping the alumina dispersion strengthened copper-based composite material ingot and then reducing it; The reduced alumina dispersion strengthened copper-based composite material ingot is hot extruded to prepare alumina dispersion strengthened copper-based composite material rods.

2. The method according to claim 1, It is characterized in that The metal having a lower reducing property than aluminum includes Ti, Ag, Ni, Sn, Cr, Zr or Zn.

3. The method according to claim 1, It is characterized in that The smelting temperature is 1100°C-1250°C.

4. The method according to claim 1, It is characterized in that The particle size of the alloy powder is less than 60 mesh, and the oxidant is Cu 2 O powder, the powder particle size of the oxidant is less than 500 meshes.

5. The method according to claim 1, It is characterized in that The cold isostatic pressing pressure is 150-300 MPa, and the holding time is 10-30 min.

6. The method according to claim 1, It is characterized in that The temperature of the vacuum pumping is 500°C-600°C, and the vacuum degree of the vacuum pumping is less than 5*10 -3 Pa, the vacuum pumping time is ≥10h.

7. The method according to claim 1, It is characterized in that The temperature of the hot isostatic pressing is 500° C.-1000° C., the pressure of the hot isostatic pressing is 30-200 MPa, and the time of the hot isostatic pressing is 1-8 hours.

8. The method according to claim 1, It is characterized in that The reducing atmosphere of the reduction is hydrogen, the reducing temperature is 50-900° C., and the reducing time is 1-16 hours.

9. The method according to claim 1, It is characterized in that The hot extrusion temperature is 700-950° C., and the extrusion ratio is 10-50.

10. An alumina dispersion strengthened copper-based composite material rod, It is characterized in that The invention comprises the following components in percentage by mass: 0.1-2.0% of aluminum oxide, 0.1-2.0% of a metal with a reducing property lower than that of aluminum, and the rest of copper.

Citation Information

Cited By

  • High-heat-resistant copper-based composite material and high-throughput preparation method and application thereof