High-temperature-resistant SiC coating material and coating preparation method
By wrapping the Si layer on the SiC surface to form SiO2, the problem of insufficient oxidation resistance of SiC coating in high-temperature environments is solved, high-temperature stability and long-life use are achieved, and it is suitable for ultra-high temperature conditions of 1500-1600℃.
Patent Information
- Application Number
- CN202411180518.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing SiC ceramic coatings have insufficient oxidation resistance under high temperature environments. Traditional binders introduce pollutants and are costly, making it difficult to meet the ultra-high temperature operating conditions of 1500-1600℃, resulting in unstable coating performance and short life.
SiC is used as the core, and Si is wrapped as a bonding phase to form a cladding layer on the surface of SiC. SiO2 is formed by depositing Si atoms through rotary fluidized beds, which not only plays a bonding role in the thermal spraying process, but also prevents SiC sintering in high temperature environments. Improves the oxidation resistance and stability of the coating.
It realizes the long-life use of SiC coating in a high temperature environment of 1500-1600℃, with a maximum service temperature of 1600℃, good bonding between the coating and the substrate, and the number of thermal shock resistance is greater than 200 times, meeting the new generation of semiconductors, aero engines and other fields. demand.
Smart Images

Figure CN119061346A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal spraying surface engineering, and in particular to a high temperature resistant SiC coating material and a coating preparation method. Background Art
[0002] SiC has excellent physical and chemical properties such as high melting point, high hardness, corrosion resistance, and oxidation resistance, especially in the range of 1800-2000℃, it has good anti-ablation performance. In the field of high-end equipment manufacturing, SiC ceramic wear-resistant coatings are widely used in microelectronics, aviation, aerospace and other fields. For example, in the semiconductor industry, for the development of third-generation semiconductor devices, SiC is the core material currently being researched and developed, and is mainly used in the production of core components such as semiconductor silicon boats.
[0003] It should be pointed out that in the process of thermal spraying coating, SiC as a ceramic hard phase must be added with a binder. The conventional binders are Co and Ni materials, which pose fatal problems to the semiconductor industry, such as easy introduction of pollutants, poor thermal stability of the coating at high temperatures, etc. At present, the actual maximum service temperature of SiC ceramic reinforced coating is 1200℃, which cannot meet the needs of the semiconductor electronics industry. It is extremely necessary to improve the high temperature and oxidation resistance of the coating. It is reported that the common methods for improving the high temperature oxidation resistance of such coatings include using laser to prepare Ni625+SiC+Ni(WC) multi-component ceramic modified high temperature oxidation resistant layer (patent number CN202310038375.6), and using thermal spraying SiC+Si+BN composite powder to prepare high temperature sealing coating, with a maximum applicable temperature of 1350°C, which can be used for aircraft engines and gas turbines (authorized patent number CN201810200025.4), but it still has the disadvantages of high cost, complex process, easy introduction of impurities, and low service temperature, and cannot be used in ultra-high temperature conditions of 1500-1600°C. Long-term use under such service conditions may cause local damage to the coating surface. Traditional SiC coating materials and their preparation methods can no longer meet such high service temperature requirements. How to improve the purity and high temperature stability of SiC coatings and determine the appropriate powder preparation technology and coating preparation process are the key to research in this field.
[0004] Therefore, it is of great practical significance to provide a raw material and a preparation method that can improve the high temperature stability of SiC coatings. Summary of the invention
[0005] The object of the present invention is to provide a high-temperature resistant SiC coating material and a coating preparation method. The high-temperature resistant SiC coating material has SiC as a core and Si as a bonding phase. Si as a bonding phase is wrapped around the outside of SiC, thereby ensuring the oxidation resistance of the coating in a high-temperature environment of 1500-1600°C; at the same time, Si atoms are deposited on the surface of SiC particles to form a coating layer, which can not only act as a bonding phase during thermal spraying, but also generate SiO2 in a high-temperature service environment to prevent the SiC-based phase from sintering and densification, so that the coating always maintains excellent performance and meets the requirements of long-life use.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a high temperature resistant SiC coating material, comprising the following components in percentage by mass: 8.0-15.0% Si, and the remainder SiC;
[0008] The high temperature resistant SiC coating material is a composite particle of SiC and Si;
[0009] The composite particles include a SiC core and a Si wrapping layer shell.
[0010] Preferably, the particle size of the composite particles is 30-50 μm, and the sphericity is 99%-100%; the thickness of the Si encapsulating layer shell is 5-8 μm.
[0011] Preferably, the purity of the composite particles is 99.9999%.
[0012] The present invention also provides a method for preparing the high temperature resistant SiC coating material described in the above technical solution, comprising the following steps:
[0013] Adding SiC seed crystals into the rotating fluidized bed, introducing SiH4, and cracking SiH4 into H2 and Si atoms under the first temperature condition;
[0014] Under the second temperature condition, the SiC seed crystal is blown up and boiled and gasified by H2 at a pressure of 0.1 MPa, and Si atoms are deposited on the surface of the SiC particles to form a Si coating layer shell for 1-2 hours, thereby obtaining composite particles with SiC as the core and Si as the coating layer shell;
[0015] The composite particles with SiC as the core and Si as the coating shell are settled to the lower end under the action of the rotating fluidized bed and are collected after being cooled to obtain the high temperature resistant SiC coating material.
[0016] Preferably, the first temperature is 550-650°C; the second temperature is 500-600°C.
[0017] The present invention also provides a high temperature resistant SiC coating comprising the high temperature resistant SiC coating material described in the above technical solution or the high temperature resistant SiC coating material obtained by the preparation method of the high temperature resistant SiC coating material described in the above technical solution.
[0018] Preferably, the high temperature resistant SiC coating is prepared by ordinary plasma spraying or supersonic plasma thermal spraying technology.
[0019] The present invention also provides a method for preparing the high temperature resistant SiC coating described in the above technical solution, comprising the following steps:
[0020] (1) drying the high temperature resistant SiC coating material;
[0021] (2) Pre-treating the substrate workpiece;
[0022] (3) spraying the high temperature resistant SiC coating material on the pretreated substrate surface by ordinary plasma spraying or supersonic plasma thermal spraying to obtain a substrate workpiece with a coating;
[0023] (4) nitriding the substrate workpiece with the coating in an N2 furnace to form a mixed phase of SiC, Si and SiN in the coating to obtain the high temperature resistant SiC coating;
[0024] The pretreatment includes grinding, roughening, cleaning and drying;
[0025] The roughening is performed by using high-purity SiC;
[0026] The spraying conditions are as follows: power 28-35 kW, cooling gas flow rate 80-100 lpm, spraying distance 80-110 mm, powder feeding rate 30-40 g / min, coating thickness 250-300 μm;
[0027] The nitriding temperature is 1100-1200° C. and the time is 200-300 minutes.
[0028] Preferably, the proportion of each phase of SiC, Si and SiN in the high temperature resistant SiC coating is 85%:5%:10% to 85%:4%:11%.
[0029] Preferably, the coating porosity of the high temperature resistant SiC coating is 3%-7%; the thickness of the high temperature resistant SiC coating is 250-350 μm; and the bonding property between the high temperature resistant SiC coating and the substrate is 23-38 MPa.
[0030] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0031] (1) Elemental Si is added to the high temperature resistant SiC coating material of the present invention, and Si is wrapped around the SiC surface as a coating shell, so as to ensure the oxidation resistance of the coating in a high temperature environment of 1500-1600°C; at the same time, Si atoms are deposited on the surface of SiC particles to form a coating layer, which can not only act as a bonding phase during the thermal spraying process, but also generate SiO2 in a high temperature service environment to prevent the SiC-based phase from sintering and densification, so that the coating always maintains excellent performance and meets the requirements of long life use.
[0032] (2) The preparation process of the high temperature resistant SiC coating material of the present invention is simple and efficient, and the formed SiC ceramic wear-resistant coating is defect-free and has good bonding with the substrate.
[0033] (3) The Si in the high-temperature resistant SiC coating material of the present invention is used as a binder to replace traditional Co and Ni materials. The high-temperature resistant high-purity coating is prepared by ordinary plasma spraying or supersonic plasma thermal spraying process. The maximum operating temperature can reach 1600°C, which is 400°C higher than the operating temperature of the existing SiC high-temperature coating. In the 1600°C thermal shock test, the number of thermal shock resistance is greater than 200 times. The coating has good matching with the substrate material, which can give full play to the high-temperature resistance advantage of ceramic materials. It has a wide range of uses in the new generation of semiconductor industry, aircraft engines and gas turbines. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the preparation process of the high temperature resistant SiC coating material of the present invention;
[0035] In the figure, 1 is SiC seed crystal, 2 is SiH4, 3 is H2 obtained by decomposing SiH4, 4 is Si atom obtained by decomposing SiH4, 5 is H2, and 6 is Si-SiC particle;
[0036] Figure 2 Schematic diagram of the preparation method of the high temperature resistant SiC coating of the present invention;
[0037] Figure 3 It is a schematic structural diagram of the high temperature resistant SiC coating of the present invention;
[0038] Figure 4 The powder microscopic morphology and energy spectrum point scanning diagram obtained by the preparation method of Example 1 of the present invention;
[0039] Figure 5 It is a microscopic morphology image and energy spectrum line scanning image of the high temperature resistant SiC coating material prepared in Example 1 of the present invention;
[0040] Figure 6 This is the result of trace impurities measured by GDMS (glow discharge mass spectrometry) on the high temperature resistant SiC coating material prepared in Example 1 of the present invention;
[0041] Figure 7 It is a microscopic morphology image and a point scanning result image of the high temperature resistant SiC coating prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0042] The present invention provides a high temperature resistant SiC coating material, comprising the following components in percentage by mass: 8.0-15.0% Si, and the remainder SiC;
[0043] The high temperature resistant SiC coating material is a composite particle of SiC and Si;
[0044] The composite particles include a SiC core and a Si wrapping layer shell.
[0045] In the present invention, the particle size of the composite particles is preferably 30 to 50 μm, more preferably 40 to 50 μm, and more preferably 40 to 45 μm;
[0046] In the present invention, the sphericity of the composite particles is preferably 99% to 100%; the thickness of the Si encapsulating layer shell is preferably 5 to 8 μm, and more preferably 6 to 8 μm.
[0047] In the present invention, the purity of the composite particles is preferably 99.9999%.
[0048] The high temperature resistant SiC coating material of the present invention uses Si as the outer shell of the wrapping layer and as the bonding phase, and uses SiC as the base phase. The thermal expansion coefficient of the SiC matches that of the high strength alloy steel substrate, and the heat resistance can reach 1500-1600°C, ensuring that the coating has an excellent thermal cycle life on the high strength alloy steel substrate.
[0049] The present invention also provides a method for preparing the high temperature resistant SiC coating material described in the above technical solution, comprising the following steps:
[0050] SiH4 is introduced into the rotating fluidized bed to crack SiH4 into H2 and Si atoms under a first temperature condition, and then SiC seed crystals are added;
[0051] Under the second temperature condition, the SiC seed crystal is blown up and boiled and gasified by H2 at a pressure of 0.1 MPa, and Si atoms are deposited on the surface of the SiC particles to form a Si coating layer shell, thereby obtaining composite particles with SiC as the core and Si as the coating layer shell;
[0052] The composite particles with SiC as the core and Si as the coating shell are settled to the lower end under the action of the rotating fluidized bed and are collected after being cooled to obtain the high temperature resistant SiC coating material.
[0053] In the present invention, the first temperature is preferably 550-650°C, more preferably 550-600°C; the second temperature is preferably 500-600°C, more preferably 550-600°C.
[0054] In the present invention, the rotation speed of the fluidized bed is preferably 500 rpm, the particle size of the SiC seed crystal is preferably 10-15 μm, and the purity is preferably 99.9999%.
[0055] In the present invention, the decomposition time of SiH4 into H2 and Si atoms is preferably 30 minutes;
[0056] In the present invention, the deposition time of the Si atoms on the surface of the SiC particles is 1 to 2 hours.
[0057] In the present invention, the different precipitation times of Si atoms on the surface of SiC particles will directly affect the thickness of the coating layer, and then affect the high-temperature stability of the subsequent SiC material. The deposition time of 1 to 2 hours specified in the present invention is more beneficial to the high-temperature reliability of the obtained SiC material.
[0058] The preparation process of the high temperature resistant SiC coating material of the present invention is simple and efficient, and the formed SiC ceramic wear-resistant coating is defect-free and has good bonding with the substrate; at the same time, Si atoms are deposited on the surface of SiC particles to form a coating layer, which can not only act as a bonding phase during the thermal spraying process, but also generate SiO2 in a high temperature service environment to prevent the SiC base phase from sintering and densification, so that the coating always maintains excellent performance and meets the requirements of long life use.
[0059] The present invention also provides a high temperature resistant SiC coating comprising the high temperature resistant SiC coating material described in the above technical solution or the high temperature resistant SiC coating material obtained by the preparation method of the high temperature resistant SiC coating material described in the above technical solution.
[0060] In the present invention, the high temperature resistant SiC coating is preferably prepared by ordinary plasma spraying or supersonic plasma thermal spraying technology.
[0061] The present invention also provides a method for preparing the high temperature resistant SiC coating described in the above technical solution, comprising the following steps:
[0062] (1) drying the high temperature resistant SiC coating material;
[0063] (2) Pre-treating the substrate workpiece;
[0064] (3) spraying the high temperature resistant SiC coating material on the pretreated substrate surface by ordinary plasma spraying or supersonic plasma thermal spraying to obtain a substrate workpiece with a coating;
[0065] (4) nitriding the substrate workpiece with the coating in an N2 furnace to form a mixed phase of SiC, Si and SiN in the coating to obtain the high temperature resistant SiC coating;
[0066] The pretreatment includes grinding, roughening, cleaning and drying;
[0067] The roughening is performed by using high-purity SiC;
[0068] The spraying conditions are as follows: power 28-35 kW, cooling gas flow rate 80-100 lpm, spraying distance 80-110 mm, powder feeding rate 30-40 g / min, coating thickness 250-300 μm;
[0069] The nitriding temperature is 1100-1200° C. and the time is 200-300 minutes.
[0070] In the present invention, the drying is preferably drying the high temperature resistant SiC coating material at 80°C for 1 hour; the roughening is preferably performed using high purity SiC. Furthermore, the roughening is performed using a sandblasting machine.
[0071] In the present invention, the cleaning is preferably performed by washing with alcohol or acetone.
[0072] In the present invention, the spraying is preferably performed by evacuating the spraying chamber to 30 mbar, backfilling it with argon gas to 50 mbar, and then spraying is performed after reaching the spraying state.
[0073] In the present invention, the spraying conditions are preferably 28-35kW power, 80-100lpm cooling gas flow, 80-110mm spraying distance, 30-40g / min powder feeding rate, and 250-300μm coating thickness; the cooling gas is preferably argon; further preferably, the power is 20-35kW, the cooling gas flow is 80-90lpm, the spraying distance is 90-110mm, the powder feeding rate is 35-40g / min, and the coating thickness is 250-270μm, and the cooling gas is preferably argon.
[0074] In the present invention, the nitriding temperature is preferably 1100-1200° C., and the time is preferably 200-300 mins, and more preferably the temperature is 1150-1200° C., and the time is 250-300 mins.
[0075] In the present invention, the proportion of each phase of SiC, Si and SiN in the high temperature resistant SiC coating is preferably 85%:5%:10% to 85%:4%:11%, wherein the SiC, Si and SiN exist in the form of three mutually doped phases.
[0076] In the present invention, the coating porosity of the high temperature resistant SiC coating is 3%-7%; the thickness of the high temperature resistant SiC coating is 250-350 μm; and the bonding property between the high temperature resistant SiC coating and the substrate is 23-38 MPa.
[0077] The Si in the high-temperature resistant SiC coating material of the present invention is used as a binder to replace traditional Co and Ni materials. The high-temperature resistant high-purity coating is prepared by ordinary plasma spraying or supersonic plasma thermal spraying process. The maximum operating temperature can reach 1600°C, which is 400°C higher than the operating temperature of the existing SiC high-temperature coating. The coating has good matching with the substrate material and can give full play to the high-temperature resistance advantage of the ceramic material. It has a wide range of uses in the new generation of semiconductor industry, aircraft engines and gas turbines.
[0078] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.
[0079] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0080] Example 1
[0081] Preparation of high temperature resistant SiC coating materials
[0082] (1) Adding SiC seed crystals with a particle size of 10 to 15 μm and a purity of 99.9999% into a fluidized bed at a rotation speed of 500 rpm;
[0083] (2) introducing SiH4 gas and cracking SiH4 at 550°C for 30 mins to form H2 and Si atoms;
[0084] (3) At a temperature of 500°C, H2 at a pressure of 0.1 MPa is introduced to boil and vaporize the SiC seed crystals, and Si atoms are deposited on the surface of the SiC seed crystal particles to form a coating shell. After deposition for 1 hour, composite particles with a particle size of 30-45 μm and a Si core and Si coating shell are formed. The composite particles with SiC as the core and Si as the coating shell settle to the lower end under the action of the rotating fluidized bed, and are collected after cooling to obtain a high-temperature resistant SiC coating material.
[0085] Example 2
[0086] Preparation of high temperature resistant SiC coating materials
[0087] (1) Adding SiC seed crystals with a particle size of 10 to 15 μm and a purity of 99.9999% into a fluidized bed at a rotation speed of 500 rpm;
[0088] (2) introducing SiH4 gas and cracking SiH4 at 650°C for 30 mins to form H2 and Si atoms;
[0089] (3) At a temperature of 600°C, H2 at a pressure of 0.1 MPa is introduced to cause the SiC seed crystals to boil and vaporize, and Si atoms are deposited on the surface of the SiC seed crystal particles to form a coating shell. After deposition for 2 hours, composite particles with a particle size of 40-50 μm and a Si core and Si as a coating shell are formed. The composite particles with SiC as the core and Si as the coating shell settle to the lower end under the action of the rotating fluidized bed, and are collected after cooling to obtain a high-temperature resistant SiC coating material.
[0090] Example 3
[0091] Preparation of high temperature resistant SiC coating
[0092] (1) The high temperature resistant SiC coating material prepared in Example 1 was dried at 80° C. for 1 h;
[0093] (2) Using a sandblasting machine, the base workpiece is ground and roughened with high-purity SiC particles, and then cleaned with alcohol, dried, installed on the sprayed workpiece, and placed in a common plasma spraying cabin;
[0094] (3) The spray chamber was evacuated to 30 mbar, and argon was used to backfill to 50 mbar to achieve the spraying state; at the same time, the spraying parameters were set as follows: power 30 kW, argon was used for cooling, argon flow rate 100 lpm, spraying distance 90 mm, powder feeding rate 30 g / min, coating thickness 250 μm, and when the temperature of the substrate workpiece dropped below 300 °C, argon was backfilled to cool to below 100 °C, and the substrate workpiece coated with the coating was taken out;
[0095] (4) The substrate workpiece with the coating is placed in a N2 furnace for nitriding. The temperature in the furnace is set to 1100°C and the nitriding time is 3.5 hours. A mixed phase of SiC, Si and SiN is formed in the coating. The proportions of SiC, Si and SiN in the high-temperature resistant SiC coating are 85%:5%:10%. Thus, a high-temperature resistant SiC coating is obtained. The thickness of the high-temperature resistant SiC coating is 250 μm, the porosity is 3.2%, and in a 1600°C thermal shock test, the thermal shock resistance is 210 times, and the bonding property with the substrate is 38 MPa.
[0096] Example 4
[0097] Preparation of high temperature resistant SiC coating
[0098] (1) The high temperature resistant SiC coating material prepared in Example 1 was dried at 80° C. for 1 h;
[0099] (2) Using a sandblasting machine, the base workpiece is ground and roughened with high-purity SiC particles, and then cleaned with acetone, dried, mounted on the sprayed workpiece, and placed in a supersonic plasma spraying chamber;
[0100] (3) The spray chamber was evacuated to 30 mbar, and argon was used to backfill to 50 mbar to achieve the spraying state; at the same time, the spraying parameters were set as follows: power 28 kW, argon was used for cooling, argon flow rate 80 lpm, spraying distance 110 mm, powder feeding rate 40 g / min, coating thickness 300 μm, and when the temperature of the substrate workpiece dropped below 300 °C, argon was backfilled to cool to below 100 °C, and the substrate workpiece coated with the coating was taken out;
[0101] (4) The substrate workpiece with the coating is placed in a N2 furnace for nitriding. The temperature in the furnace is set to 1200°C and the nitriding time is 5 hours, so that a mixed phase of SiC, Si and SiN is formed in the coating. The proportions of SiC, Si and SiN in the high-temperature resistant SiC coating are 85%:4%:11%, thereby obtaining a high-temperature resistant SiC coating. The thickness of the high-temperature resistant SiC coating is 300 μm, the porosity is 6%, and in a 1600°C thermal shock test, the thermal shock resistance is 230 times, and the bonding property with the substrate is 23 MPa.
[0102] Based on the above, it can be known that the high temperature resistant SiC obtained in the present invention has a thermal shock resistance of more than 200 times in a 1600°C thermal shock test, and the bonding strength between the high temperature resistant SiC coating and the substrate is 23-38MPa. It has excellent thermal stability at high temperatures and excellent bonding strength with the substrate.
[0103] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high temperature resistant SiC coating material, characterized in that: The invention comprises the following components in percentage by mass: 8.0-15.0% Si, and the balance is SiC; The high temperature resistant SiC coating material is a composite particle of SiC and Si; The composite particles include a SiC core and a Si wrapping layer shell.
2. The high temperature resistant SiC coating material according to claim 1, characterized in that: The particle size of the composite particles is 30-50 μm, and the sphericity is 99%-100%; the thickness of the outer shell of the Si wrapping layer is 5-8 μm.
3. The high temperature resistant SiC coating material according to claim 1, characterized in that: The purity of the composite particles is 99.9999%.
4. A method for preparing a high temperature resistant SiC coating material according to any one of claims 1 to 3, characterized in that: The following steps are involved: Adding SiC seed crystals into the rotating fluidized bed, introducing SiH4, and cracking SiH4 into H2 and Si atoms under the first temperature condition; Under the second temperature condition, the SiC seed crystal is blown up and boiled and gasified by H2 at a pressure of 0.1 MPa, and Si atoms are deposited on the surface of the SiC particles to form a Si coating layer shell for 1-2 hours, thereby obtaining composite particles with SiC as the core and Si as the coating layer shell; The composite particles with SiC as the core and Si as the coating shell are settled to the lower end under the action of the rotating fluidized bed and are collected after being cooled to obtain the high temperature resistant SiC coating material.
5. The method for preparing a high temperature resistant SiC coating material according to claim 4, characterized in that: The first temperature is 550-650°C; the second temperature is 500-600°C.
6. A high temperature resistant SiC coating comprising the high temperature resistant SiC coating material according to any one of claims 1 to 3.
7. The high temperature resistant SiC coating according to claim 6, characterized in that: The high temperature resistant SiC coating is prepared by ordinary plasma spraying or supersonic plasma thermal spraying technology.
8. A method for preparing a high temperature resistant SiC coating according to claim 6, characterized in that: The following steps are involved: (1) drying the high temperature resistant SiC coating material; (2) Pre-treating the substrate workpiece; (3) using ordinary plasma spraying or supersonic plasma thermal spraying to spray the high temperature resistant SiC coating material on the pretreated substrate surface to obtain a substrate workpiece with a coating; (4) nitriding the substrate workpiece with the coating in an N2 furnace to form a mixed phase of SiC, Si and SiN in the coating to obtain the high temperature resistant SiC coating; The pretreatment includes grinding, roughening, cleaning and drying; The roughening is performed by using high-purity SiC; The spraying conditions are as follows: power 28-35 kW, cooling gas flow rate 80-100 lpm, spraying distance 80-110 mm, powder feeding rate 30-40 g / min, coating thickness 250-300 μm; The nitriding temperature is 1100-1200° C. and the time is 200-300 minutes.
9. The method for preparing a high temperature resistant SiC coating according to claim 6, characterized in that: The proportions of SiC, Si and SiN phases in the high temperature resistant SiC coating are 85%:5%:10% to 85%:4%:11%.
10. The method for preparing a high temperature resistant SiC coating according to claim 6, characterized in that: The porosity of the high temperature resistant SiC coating is 3%-7%; the thickness of the high temperature resistant SiC coating is 250-350 μm; and the bonding strength between the high temperature resistant SiC coating and the substrate is 23-38 MPa.
Citation Information
Patent Citations
Preparation method and applications of cold-wall fluidized bed
CN103172381A
Composite coating carbon / carbon composite material crucible and preparation method thereof
CN103553711A
Core-shell structure nanometer composite particle as well as preparation method and preparation device thereof
CN108675300A
Method for depositing an in situ coating onto thermally and chemically loaded components of a fluidized bed reactor for producing high-purity polysilicon
CN108699683A