Hydrogen-doped zinc oxide visible-near infrared transparent conductive film and preparation method thereof
A hydrogen-doped zinc oxide film addresses the limitations of indium-based films by optimizing carrier concentration and mobility through magnetron sputtering, achieving high transmittance and conductivity across visible and near-infrared bands, suitable for diverse applications.
Patent Information
- Application Number
- CN202411045583.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-01
Smart Images

Figure CN119061368A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of transparent conductive films, and more specifically, relates to a hydrogen-doped zinc oxide visible-near infrared transparent conductive film and a preparation method thereof. Background Art
[0002] Transparent conductive films are widely used in the field of optoelectronic devices because of their high optical transmittance and excellent conductivity. At present, transparent conductive films suitable for the visible light band (0.38-0.78μm) are relatively mature, and transparent conductive oxide films represented by tin-doped indium oxide (In2O3:Sn, ITO) have been commercialized and occupy a considerable market share. With the further innovation of military fields such as photoelectric detection and camouflage, as well as civilian fields such as solar cells and smart windows, transparent conductive films must not only meet high visible light transparency, but also ensure good transmittance in the near-infrared light region (0.78-2.50μm) (the transmittance is often required to be no less than 60%). Although the transmittance of commercial ITO materials in the visible light band can exceed 70%, the transmittance in the near-infrared band is usually less than 50%. This defect limits its application in scenes with high requirements for near-infrared transparency.
[0003] According to the Drude model, the transparent window of metal oxide conductive materials is mainly determined by the semiconductor band edge absorption and the plasma co-oscillation effect, among which the plasma resonance wavelength determines the upper wavelength limit of the material's transparent window. ITO's own high carrier concentration makes its plasma resonance wavelength close to the visible light region, resulting in low near-infrared transmittance. Appropriately reducing the carrier concentration can cause the plasma resonance wavelength to redshift, thereby improving the near-infrared transmittance. However, a decrease in carrier concentration will have an adverse effect on the conductivity of the material. When the carrier concentration remains unchanged, the higher the carrier mobility, the stronger the conductivity of the material. In order to simultaneously optimize the near-infrared transmittance and conductivity of metal oxides, it is key to improve the carrier mobility while controlling the appropriate carrier concentration. In the prior art, researchers used molybdenum to replace tin and developed molybdenum-doped indium oxide. The mobility of this material is about twice that of ITO with the same carrier concentration, and the conductivity can reach 1.25×10 4 S cm -1 , the transmittance at a wavelength of 1500nm exceeds 60% (JEN Swallow, BAD Williamson and et al, Materials Horizons, 2020, 7, 236-243). Chinese patent specification CN116072326A also discloses a method for preparing a transparent conductive film using a multi-oxide doped indium oxide target such as titanium oxide and hafnium oxide. The mobility of the obtained film material is 80.5-82.5cm 2 ·V-1 ·s -1 , achieving a transmittance of 90.0-90.5% at 0.40-1.20μm, while meeting the requirements of high visible-near infrared transmittance and high mobility.
[0004] The near-infrared transparent conductive films mentioned above are all doped with indium oxide as the matrix, and most of the commonly used transparent conductive films are also based on indium oxide materials. However, the main raw material metal indium in indium oxide is a scarce resource. With the sharp increase in demand for indium in industries such as new energy, consumer electronics and optical communications, and the restrictions on the mining of indium mines due to environmental protection policies, the price fluctuations and stable supply of indium will seriously restrict the large-scale production of indium oxide-based transparent conductive materials. In view of this, the design and preparation of indium-free visible-near-infrared transparent conductive materials with high mobility and low cost is of great significance to the development of optoelectronic technology. Summary of the invention
[0005] In view of the above defects or improvement needs of the prior art, the purpose of the present invention is to provide a hydrogen-doped zinc oxide visible-near infrared transparent conductive film and a preparation method thereof, wherein by controlling the composition and crystallinity of the film, the carrier concentration of the film is controlled, and the mobility is improved, which can effectively solve the technical problem that the traditional transparent conductive film is difficult to be compatible with high near-infrared transmittance and high conductivity. The transparent conductive film obtained by the present invention has a transmittance of not less than 60% in the visible light band (0.38-0.78 μm), a transmittance of not less than 70% in the near-infrared band (0.78-2.50 μm), and good conductivity. In addition, since the present invention obtains hydrogen-doped zinc oxide, the use of indium is avoided, which can overcome the high cost of indium-containing transparent conductive films. At the same time, the simple magnetron sputtering process (especially the room temperature magnetron sputtering process) can also make the visible-near infrared transparent conductive film match more application scenarios.
[0006] To achieve the above object, according to one aspect of the present invention, a hydrogen-doped zinc oxide visible-near infrared transparent conductive film is provided, characterized in that the preparation method thereof is as follows: using magnetron sputtering, zinc oxide as a target material, and an inert gas mixed with hydrogen and / or water vapor as a sputtering gas, by controlling the total volume proportion of hydrogen and water vapor in the sputtering gas to 2-10%, and controlling the sputtering gas pressure to 0.2-1.2 Pa, and the sputtering power density to 3.0-5.0 W·cm -2 , a hydrogen-doped zinc oxide visible-near infrared transparent conductive film can be deposited on the substrate;
[0007] The transmittance of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film in the 0.38μm-0.78μm band is not less than 60%, and the transmittance in the 0.78μm-2.50μm band is not less than 70%. The conductivity at room temperature is higher than 0.8×103 S cm -1 .
[0008] As a further preferred embodiment of the present invention, at room temperature, the carrier mobility of the transparent conductive film is higher than 35 cm 2 ·V -1 ·s -1 , square resistance is less than 30Ω·sq -1 .
[0009] As a further preferred embodiment of the present invention, the transparent conductive film has a thickness of 100 to 800 nm.
[0010] According to another aspect of the present invention, the present invention provides a method for preparing the above hydrogen-doped zinc oxide visible-near infrared transparent conductive film, characterized in that it comprises the following steps:
[0011] S1. Prepare zinc oxide target and clean substrate;
[0012] S2. The substrate and the zinc oxide target are respectively mounted on the substrate base and the target base of the magnetron sputtering equipment;
[0013] S3. The magnetron sputtering equipment is evacuated until the vacuum degree of the equipment chamber drops to 1×10 -5 ~1×10 -3 When the pressure is 0.2 Pa, an inert gas mixed with hydrogen and / or water vapor is introduced into the chamber, and the total volume proportion of hydrogen and water vapor in the mixed gas is controlled to be 2-10%, and the sputtering pressure is controlled to be 0.2-1.2 Pa, and the sputtering power density is controlled to be 3.0-5.0 W·cm -2 By performing magnetron sputtering in this way, a hydrogen-doped zinc oxide visible-near infrared transparent conductive film can be deposited on the substrate.
[0014] As a further preferred embodiment of the present invention, the sputtering time is 30 to 120 minutes, and the thickness of the corresponding transparent conductive film is 100 to 800 nm.
[0015] As a further preferred embodiment of the present invention, the inert gas is at least one of argon and helium.
[0016] As a further preferred embodiment of the present invention, during the magnetron sputtering process, the substrate temperature is 20-60°C.
[0017] According to another aspect of the present invention, the present invention provides an application of the above-mentioned hydrogen-doped zinc oxide visible-near infrared transparent conductive film as a transparent conductive film in the 0.78μm to 2.50μm band, characterized in that the transmittance of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film in the 0.78μm to 2.50μm band is not less than 70%.
[0018] According to another aspect of the present invention, the present invention provides an application of the above-mentioned hydrogen-doped zinc oxide visible-near infrared transparent conductive film as a transparent conductive film in the 0.38μm to 0.78μm band, characterized in that the transmittance of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film in the 0.38μm to 0.78μm band is not less than 60%.
[0019] Through the above technical scheme conceived by the present invention, compared with the prior art, the present invention designs a hydrogen-doped zinc oxide film, and controls the composition and crystallinity of the hydrogen-doped zinc oxide film, thereby controlling the carrier concentration of the film and improving the mobility. The obtained transparent conductive film has a transmittance of not less than 60% in the visible light band (0.38-0.78 μm), a transmittance of not less than 70% in the near-infrared band (0.78-2.50 μm), and a conductivity of more than 0.8×10 3 S cm -1 、Square resistance lower than 30Ω·sq -1 The hydrogen-doped zinc oxide visible-near infrared transparent conductive film of the present invention is prepared by a magnetron sputtering process, wherein zinc oxide is used as a target material and a mixed gas containing hydrogen and / or water vapor is used as a sputtering gas, and the hydrogen doping concentration is strictly controlled (by strictly controlling the total volume ratio of the sputtering gas hydrogen and water vapor to 2-10%), the sputtering pressure is strictly controlled to 0.2-1.2 Pa, and the sputtering power density is strictly controlled to 3.0-5.0 W·cm -2 , which can effectively control the hydrogen doping amount and crystallinity of the hydrogen-doped zinc oxide film. The obtained hydrogen-doped zinc oxide has a hexagonal wurtzite structure and good crystallinity, ensuring the transmittance and conductivity in the near-infrared band.
[0020] Specifically, the present invention can achieve the following beneficial effects:
[0021] 1. The mobility of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film obtained by the present invention exceeds 35 cm 2 ·V -1 ·s -1 , significantly better than other doped zinc oxide materials (mobility is generally 1 to 30 cm 2 ·V -1 ·s -1 ), so it has excellent near-infrared transmittance and electrical conductivity, specifically, its transmittance in the near-infrared band (0.78-2.50 μm) is not less than 70%, and its electrical conductivity is higher than 0.8×10 3 S cm -1 、Square resistance lower than 30Ω·sq -1 .
[0022] Meanwhile, the transparent conductive film obtained by the present invention has a transmittance of not less than 60% in the visible light band (0.38-0.78 μm), and can be used as a transparent conductive film in both the visible light band and the near infrared band.
[0023] 2. The hydrogen-doped zinc oxide visible-near infrared transparent conductive film of the present invention does not contain indium, and its main component is Zn element, which is low in price and abundant in reserves, and can effectively reduce the raw material cost of the transparent conductive film.
[0024] 3. The preparation method provided by the present invention is based on magnetron sputtering technology, which is simple in process and suitable for large-scale production applications. During the magnetron sputtering process, the substrate temperature can be 20-60°C, especially at room temperature (the substrate does not need additional heating), and is suitable for a variety of substrates including flexible materials with low high temperature tolerance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The following are scanning electron microscope (SEM) images of the surface and cross section of the hydrogen-doped zinc oxide transparent conductive film prepared in Example 1 of the present invention. Figure 1 (a) corresponds to the surface SEM image, Figure 1 (b) corresponds to the cross-sectional SEM image.
[0026] Figure 2 This is an X-ray diffraction (XRD) diagram of the hydrogen-doped zinc oxide transparent conductive film prepared in Example 1 of the present invention.
[0027] Figure 3 This is a transmission spectrum of the hydrogen-doped zinc oxide transparent conductive film prepared in Example 1 of the present invention. The data of the "ZnO:H / soda-lime glass" curve is measured with air as the baseline, while the data of the "ZnO:H" curve is measured with blank soda-lime glass as the baseline.
[0028] Figure 4 This is a scanning electron microscope (SEM) image of the surface of the hydrogen-doped zinc oxide transparent conductive film in Example 2 of the present invention.
[0029] Figure 5 This is a transmission spectrum diagram of the hydrogen-doped zinc oxide transparent conductive film in Example 2 of the present invention.
[0030] The data of the “ZnO:H / soda-lime glass” curve are measured with air as the baseline, while the data of the “ZnO:H” curve are measured with blank soda-lime glass as the baseline.
[0031] Figure 6 This is a scanning electron microscope (SEM) image of the surface of the hydrogen-doped zinc oxide transparent conductive film in Example 3 of the present invention.
[0032] Figure 7 This is a transmission spectrum diagram of the hydrogen-doped zinc oxide transparent conductive film in Example 3 of the present invention.
[0033] The data of the “ZnO:H / PET” curve are measured with air as the baseline, while the data of the “ZnO:H” curve are measured with blank PET as the baseline. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0035] The soda-lime glass used in the following examples was purchased from Zhuhai Kaiwei Optoelectronics Technology Co., Ltd., with a specific model of KV-SLG-001-100100 and a thickness of 1.1 mm; the PET film used was purchased from Shenzhen Hongsheng Plastic Co., Ltd., with a specific model of HS-PET02 and a thickness of 50 μm.
[0036] The present invention uses a magnetron sputtering method to prepare a hydrogen-doped zinc oxide visible-near infrared transparent conductive film, which can be operated according to the following steps:
[0037] S1, ultrasonically clean the substrate and blow dry it with nitrogen;
[0038] S2, installing the substrate and the zinc oxide target on the substrate base and the target base of the magnetron sputtering equipment respectively;
[0039] S3, start the vacuum system of the magnetron sputtering equipment, and wait until the vacuum degree of the equipment chamber drops to 1×10 -5 ~1×10 -3 When Pa, a mixed gas containing hydrogen and / or water vapor is introduced into the chamber, and the chamber pressure is controlled by adjusting the flow rate of the mixed gas;
[0040] S4, setting the sputtering power density, igniting the sputtering gas, adjusting the sputtering time, and depositing the hydrogen-doped zinc oxide visible-near infrared transparent conductive film on the surface of the substrate.
[0041] The following are specific embodiments:
[0042] Example 1
[0043] The soda lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. The soda lime glass and intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 8×10 -5 Pa. A mixture of hydrogen and argon is introduced into the chamber, with hydrogen accounting for 10% of the volume. The flow rate of the hydrogen and argon mixture is adjusted to make the chamber pressure 0.5 Pa. The sputtering power density is set to 4.0 W cm -2 , sputtering for 60 minutes, substrate temperature 30 ° C, to obtain a hydrogen-doped zinc oxide transparent conductive film with a thickness of 518.8nm ( Figure 1 ). Figure 2 Figure 2 is an XRD diagram of a hydrogen-doped zinc oxide transparent conductive film, which has a hexagonal wurtzite structure with good crystallinity. Figure 3 As shown in the figure, the transmittance of the hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 64% and 99%, and the transmittance in the near-infrared band is between 70% and 99%. The Hall effect test results show that the mobility, conductivity and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 47.4 cm 2 ·V -1 ·s -1 , 1.07×10 3 S cm -1 , 16Ω·sq -1 .
[0044] Example 2
[0045] The soda-lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. The soda-lime glass and intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 5×10 -4 Pa. A mixture of water vapor and argon is introduced into the chamber, with water vapor accounting for 10% of the volume. The flow rate of the water vapor and argon mixture is adjusted to make the chamber pressure 0.2 Pa. The sputtering power density is set to 5.0 W cm -2 , sputtering for 30 minutes, substrate temperature 35 ° C, the obtained hydrogen-doped zinc oxide transparent conductive film morphology is as follows Figure 4 .like Figure 5 As shown, the transmittance of hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 68% and 99%, and the transmittance in the near infrared band is between 82% and 99%. The Hall effect test results show that the mobility, conductivity and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 42.7 cm 2 ·V -1 ·s -1 , 1.01×103 S cm -1 , 28Ω·sq -1 .
[0046] Example 3
[0047] The polyethylene terephthalate (PET) film was ultrasonically cleaned in ethanol and deionized water for 10 minutes, and then the surface was dried with nitrogen. The PET film and the intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 8×10 -4 Pa. A mixture of hydrogen and argon is introduced into the chamber, with hydrogen accounting for 5% by volume. The flow rate of the hydrogen and argon mixture is adjusted to make the chamber pressure 0.8 Pa. The sputtering power density is set to 3.5 W cm -2 , sputtering for 75 minutes, substrate temperature 25 ° C, the obtained hydrogen-doped zinc oxide transparent conductive film morphology is as follows Figure 6 .like Figure 7 As shown in the figure, the transmittance of the hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 60% and 99%, and the transmittance in the near-infrared band is between 82% and 99%. The Hall effect test results show that the mobility, conductivity and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 41.6 cm 2 ·V -1 ·s -1 , 1.04×10 3 S cm -1 , 18Ω·sq -1 .
[0048] Example 4
[0049] Soda lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. Soda lime glass and aluminum-doped zinc oxide ceramic target (aluminum doping mass fraction was 2%) were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 5×10 -4 Pa. A mixture of hydrogen and argon is introduced into the chamber, with hydrogen accounting for 2% by volume. The flow rate of the hydrogen and argon mixture is adjusted to make the chamber pressure 0.75 Pa. The sputtering power density is set to 4 W cm -2 , sputtering for 70 minutes, substrate temperature 35°C, the transmittance of the hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 70% and 99%, and the transmittance in the near-infrared band is between 70% and 99.9%. The Hall effect test results show that the mobility, conductivity and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 35.1cm 2 ·V -1 ·s -1, 1.04×10 3 S cm -1 , 24Ω·sq -1 .
[0050] Example 5
[0051] The soda-lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. The soda-lime glass and intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 6×10 -4 Pa. A mixture of hydrogen and argon is introduced into the chamber, with hydrogen accounting for 8% by volume. The flow rate of the hydrogen and argon mixture is adjusted to make the chamber pressure 1.2 Pa. The sputtering power density is set to 4.5 W cm -2 , sputtering for 90 minutes, substrate temperature 40°C, the transmittance of the hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 70% and 99%, and the transmittance in the near-infrared band is between 70% and 99.5%. The Hall effect test results show that the mobility, conductivity and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 36.5cm 2 ·V -1 ·s -1 , 1.06×10 3 S cm -1 , 28Ω·sq -1 .
[0052] Example 6
[0053] The soda-lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. The soda-lime glass and intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 1×10 -4 Pa. A mixture of hydrogen and argon is introduced into the chamber, with hydrogen accounting for 10% of the volume. The flow rate of the hydrogen and argon mixture is adjusted to make the chamber pressure 0.8 Pa. The sputtering power density is set to 3.0 W cm -2 , sputtering for 120 minutes, substrate temperature 40°C, the transmittance of the hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 77% and 90%, and the transmittance in the near-infrared band is between 75% and 90%. The Hall effect test results show that the mobility, conductivity and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 44.4cm 2 ·V -1 ·s -1 , 0.89×10 3 S cm -1 , 29Ω·sq-1 .
[0054] Comparative Example 1
[0055] The soda lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. The soda lime glass and intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 8×10 -5 Pa. Introduce argon gas into the chamber and adjust the argon gas flow rate to make the chamber pressure 0.8 Pa. Set the sputtering power density to 4.0 W cm -2 , sputtering for 60 minutes, substrate temperature 30°C, the transmittance of the obtained zinc oxide transparent film in the visible light band is between 60% and 99%, and the transmittance in the near infrared band is between 85% and 99%. However, the sheet resistance of the zinc oxide transparent film is greater than 3×10 5 Ω·sq -1 .
[0056] Comparative Example 2
[0057] The soda-lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. The soda-lime glass and intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 5×10 -5 Pa. A mixture of hydrogen and argon is introduced into the chamber, with hydrogen accounting for 10% of the volume. The flow rate of the hydrogen and argon mixture is adjusted to make the chamber pressure 1.6 Pa. The sputtering power density is set to 5.0 W cm -2 , sputtering for 30 minutes, substrate temperature 30°C, the transmittance of the hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 72% and 99%, and the transmittance in the near-infrared band is between 78% and 99%. However, the Hall effect test results show that the mobility, conductivity, and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 13.67 cm 2 ·V -1 ·s -1 、335S·cm -1 、138Ω·sq -1 .
[0058] Comparative Example 3
[0059] The soda-lime glass was ultrasonically cleaned in acetone, ethanol, and deionized water for 10 minutes, and then the surface was dried with nitrogen. The soda-lime glass and intrinsic zinc oxide ceramic target were installed on the substrate base and target base of the magnetron sputtering equipment. The vacuum system of the magnetron sputtering equipment was turned on and vacuum was started until the chamber vacuum reached 5×10 -5Pa. A mixture of hydrogen and argon is introduced into the chamber, with hydrogen accounting for 10% of the volume. The flow rate of the hydrogen and argon mixture is adjusted to make the chamber pressure 0.8 Pa. The sputtering power density is set to 2.5 W cm -2 , sputtering for 30 minutes, substrate temperature 30°C, the transmittance of the hydrogen-doped zinc oxide transparent conductive film in the visible light band is between 60% and 99%, and the transmittance in the near-infrared band is between 90% and 95%. However, the Hall effect test results show that the mobility, conductivity, and square resistance of the hydrogen-doped zinc oxide transparent conductive film are 0.18 cm 2 ·V -1 ·s -1 、7.83S·cm -1 , 1.12×10 4 Ω·sq -1 .
[0060] The above embodiments are only examples. For example, in addition to intrinsic zinc oxide, the target material can also be zinc oxide doped with other trace metal elements (such as aluminum, titanium, tungsten, molybdenum, etc., with the doping mass fraction not exceeding 2%); for example, during magnetron sputtering, the substrate temperature can also use other temperatures in the range of 20 to 60°C.
[0061] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A hydrogen-doped zinc oxide visible-near infrared transparent conductive film, It is characterized in that The preparation method is as follows: using magnetron sputtering, zinc oxide as a target material, and an inert gas mixed with hydrogen and / or water vapor as a sputtering gas, by controlling the total volume proportion of hydrogen and water vapor in the sputtering gas to 2-10%, and controlling the sputtering gas pressure to 0.2-1.2 Pa, the sputtering power density to 3.0-5.0 W·cm -2 , a hydrogen-doped zinc oxide visible-near infrared transparent conductive film can be deposited on the substrate; The transmittance of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film in the 0.38μm-0.78μm band is not less than 60%, and the transmittance in the 0.78μm-2.50μm band is not less than 70%. The conductivity at room temperature is higher than 0.8×10 3 S cm -1 .
2. The hydrogen-doped zinc oxide visible-near infrared transparent conductive film as claimed in claim 1, It is characterized in that At room temperature, the carrier mobility of the transparent conductive film is higher than 35 cm 2 ·V -1 ·s -1 , square resistance is less than 30Ω·sq -1 .
3. The hydrogen-doped zinc oxide visible-near infrared transparent conductive film as claimed in claim 1, It is characterized in that The transparent conductive film has a thickness of 100-800 nm.
4. The method for preparing the hydrogen-doped zinc oxide visible-near infrared transparent conductive film according to any one of claims 1 to 3, It is characterized in that The steps include: S1. Prepare zinc oxide target and clean substrate; S2. The substrate and the zinc oxide target are respectively mounted on the substrate base and the target base of the magnetron sputtering equipment; S3. The magnetron sputtering equipment is evacuated until the vacuum degree of the equipment chamber drops to 1×10 -5 ~1×10 - 3 When the pressure is 0.2 Pa, an inert gas mixed with hydrogen and / or water vapor is introduced into the chamber, and the total volume proportion of hydrogen and water vapor in the mixed gas is controlled to be 2-10%, and the sputtering pressure is controlled to be 0.2-1.2 Pa, and the sputtering power density is controlled to be 3.0-5.0 W·cm -2 By performing magnetron sputtering in this way, a hydrogen-doped zinc oxide visible-near infrared transparent conductive film can be deposited on the substrate.
5. The preparation method according to claim 4, It is characterized in that The sputtering time is 30 to 120 minutes, and the thickness of the corresponding transparent conductive film is 100 to 800 nm.
6. The preparation method according to claim 4, It is characterized in that The inert gas is at least one of argon and helium.
7. The preparation method according to claim 4, It is characterized in that During magnetron sputtering, the substrate temperature is 20-60°C.
8. Use of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film as claimed in any one of claims 1 to 3 as a transparent conductive film in the wavelength range of 0.78 μm to 2.50 μm, It is characterized in that The transmittance of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film in the waveband of 0.78 μm to 2.50 μm is not less than 70%.
9. Use of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film as claimed in any one of claims 1 to 3 as a transparent conductive film in the wavelength range of 0.38 μm to 0.78 μm, It is characterized in that The transmittance of the hydrogen-doped zinc oxide visible-near infrared transparent conductive film in the waveband of 0.38 μm to 0.78 μm is not less than 60%.
Citation Information
Patent Citations
Direct preparation method of textured zinc oxide transparent electroconductive film
CN102242345A
Method for improving chemical stability of zinc oxide transparent electric conduction film
CN107217232A
Transparent conductive film and production of photoelectric conversion semiconductor device
JP1995106615A
Substrate with transparent electrode, and method of manufacturing the same
JP2011009069A
Transparent and conductive zinc oxide film with low growth temperature
US20020028571A1