Ceramic coating for corrosion prevention of neodymium-iron-boron device and preparation method of ceramic coating
Patent Information
- Application Number
- CN202411175092.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, when preparing ceramic film layers, the vacuum plating method is low in efficiency and the bonding force and corrosion resistance of the ceramic film layers with the neodymium iron boron matrix are insufficient, making it difficult to meet the corrosion protection requirements of neodymium iron boron magnets under humid and heat conditions.
The ceramic coating is formed by vacuum room temperature spraying. By sandblasting the neodymium iron boron matrix and limiting its surface roughness, it is deposited with ceramic powder of a specific particle size to form a layered microstructure to improve the coating and matrix. bonding force and overall uniformity.
It significantly improves the corrosion resistance of ceramic coatings, enhances the bonding force with neodymium iron boron matrix, improves the surface flatness and high temperature and high pressure resistance of the coating, and ensures the overall corrosion resistance of neodymium iron boron magnets.
Smart Images

Figure CN119061391A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion coatings and relates to a ceramic coating for the anti-corrosion of NdFeB devices and a preparation method thereof. Background Art
[0002] NdFeB magnets are widely used in wind power, motors, smart consumer electronics and other industries due to their excellent comprehensive magnetic properties. However, NdFeB magnets have poor chemical stability and are prone to oxidation during use. When exposed to hot and humid conditions, they are prone to severe electrochemical corrosion, so they need to be treated with surface anti-corrosion.
[0003] At present, conventional methods for surface anti-corrosion treatment of NdFeB magnets can be divided into: electroplating, chemical plating, chemical conversion film, electrophoresis and vacuum plating, etc., to obtain film layers containing metals or alloys, polymer coatings, chemical conversion film layers and composite coatings. Among them, ceramic film layers have the advantages of corrosion resistance, high hardness, high temperature resistance, and good thermal conductivity. Vacuum-plated ceramic film layers are increasingly used as corrosion-resistant film layers for NdFeB magnets. However, the vacuum plating method (eg: PVD (physical vapor deposition), CVD (chemical vapor deposition)) deposits in units of atoms or molecules and is more used in thin film preparation. When the vacuum plating method is used to prepare the ceramic film layer, the speed of forming the film layer is very slow and the production efficiency is low.
[0004] Therefore, in the art, it is desired to develop a ceramic coating for corrosion protection of NdFeB devices, which has high preparation efficiency, good bonding with the NdFeB substrate, good surface flatness, and excellent corrosion resistance. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a ceramic coating for corrosion protection of NdFeB devices and a preparation method thereof.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a ceramic coating for corrosion protection of NdFeB devices, which is characterized by a scanning electron microscope. When the magnification is 1000-7000 times (for example, 1000 times, 1500 times, 2000 times, 2500 times, 3000 times, 3500 times, 4000 times, 4500 times, 5000 times, 5500 times, 6000 times, 6500 times, 7000 times, etc.), it can be observed that the ceramic coating has a layered stacked microstructure.
[0008] The ceramic coating for corrosion protection of NdFeB devices provided by the present invention has a layered stacked microstructure. The existence of this structure enables the coating to have both good overall uniformity and good corrosion resistance.
[0009] Preferably, the ceramic coating comprises any one of yttrium oxide, aluminum oxide, silicon oxide, aluminum nitride, silicon nitride, and zirconium oxide, or a combination of at least two thereof.
[0010] Preferably, the thickness of the ceramic coating is 20-200 μm, for example, 20 μm, 25 μm, 30 μm, 40 μm, 45 μm, 50 μm, 54 μm, 58 μm, 60 μm, 65 μm, 70 μm, 80 μm, 90 μm, 100 μm, 120 μm, 150 μm, 165 μm, 180 μm, 200 μm, etc.
[0011] Preferably, the surface roughness (R a ) is 2.1-3.2 μm, for example, 2.1 μm, 2.15 μm, 2.2 μm, 2.3 μm, 2.5 μm, 2.8 μm, 3.0 μm, 3.05 μm, 3.1 μm, 3.2 μm, etc. In the present invention, the surface roughness test method of the ceramic coating is: measuring the average value of multiple groups (such as ten groups) of roughness at different sampling areas of the ceramic coating to be tested. The surface roughness test method of the NdFeB substrate described later is the same and will not be repeated one by one.
[0012] Preferably, the neutral salt spray resistance test duration of the ceramic coating is ≥340h, such as 340h, 348h, 360h, 372h, 384h, 408h, 420h, 480h, 540h, 600h, 840h, 1020h, etc. In the present invention, the test method for the neutral salt spray resistance test duration is: the corrosion resistance of the workpiece to be tested is tested by a neutral salt spray test, and the specific test conditions are: the workpiece to be tested is placed in a specific test box, and a salt water containing 50±5g / L of sodium chloride and a pH value of 6.5-7.2 is sprayed through a spray device, and the salt spray is allowed to settle on the workpiece to be tested, and the surface corrosion state is observed every 12h. When corrosion occurs, the test is terminated and the corresponding duration is recorded.
[0013] Preferably, the duration of the moisture and heat resistance test of the ceramic coating is ≥192h, such as 192h, 196h, 204h, 216h, 228h, 240h, 264h, 288h, 324h, etc. In the present invention, the test method for the moisture and heat resistance test duration is: place the workpiece to be tested in a closed environment at 120±2°C and 100%RH, observe its rust condition every 12h, and when rust occurs, end the test and record the corresponding duration.
[0014] Preferably, the bonding strength between the ceramic coating and the surface of the NdFeB substrate is ≥20MPa, such as 20MPa, 22MPa, 24MPa, 26MPa, 28MPa, 30MPa, 32MPa, 34MPa, 36MPa, 38MPa, 40MPa, etc. In the present invention, the bonding strength between the ceramic coating and the surface of the NdFeB substrate is tested by a pulling test, and the bonding strength is the average bonding strength of multiple groups (such as ten groups) of pulling test tests.
[0015] In a second aspect, the present invention provides a method for preparing a ceramic coating for corrosion protection of NdFeB devices as described in the first aspect, the preparation method comprising the following steps:
[0016] (1) Matrix pretreatment: grinding, chamfering, sandblasting and pickling of the NdFeB matrix;
[0017] (2) Vacuum room temperature spraying: using a vacuum room temperature spraying method to deposit ceramic powder on the surface of the NdFeB substrate after pickling obtained in step (1), to obtain the ceramic coating for corrosion protection of NdFeB devices;
[0018] The surface roughness (R a ) is 1.3-3.0μm, for example, 1.3μm, 1.4μm, 1.6μm, 1.8μm, 2.0μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, 3.0μm, etc.
[0019] The particle size of the ceramic powder in step (2) is 100-300 nm, for example, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, etc.
[0020] The present invention adopts a vacuum room temperature spraying process to form a ceramic coating in the field of NdFeB for the first time. The formed ceramic coating has a layered stacked microstructure. In the process of forming the coating, the substrate is sandblasted and the surface roughness after sandblasting is limited, and the particle size of the ceramic powder is controlled within a specific range. This improves the bonding strength between the coating and the substrate, improves the overall uniformity of the coating, and improves the corrosion resistance of the corners of the substrate, thereby ensuring the overall corrosion resistance of the NdFeB magnet.
[0021] In the present invention, during the pre-treatment of the NdFeB substrate, by adding a sandblasting process and limiting the surface roughness of the NdFeB substrate after sandblasting and pickling to within the range of 1.3-3.0 μm, the bonding strength between the ceramic film layer and the substrate can be improved, and the overall uniformity of the coating can be improved. If the surface roughness of the NdFeB substrate after pickling is less than 1.3 μm, the good bonding strength between the ceramic coating and the substrate cannot be guaranteed. If the surface roughness of the NdFeB substrate after pickling is greater than 3.0 μm, the surface flatness of the ceramic coating will be affected.
[0022] Since the NdFeB matrix is prepared by powder metallurgy and has certain porosity on its surface, in order to improve the bonding force between the ceramic powder and the surface of the NdFeB matrix, and to prepare a micron-level ceramic coating and ensure the density of the ceramic coating, the present invention limits the particle size of the ceramic powder to 100-300nm. If the particle size is less than 100nm, on the one hand, the particle size of the ceramic powder is difficult to control during the manufacturing process, and the formed ceramic coating has poor uniformity. Moreover, the particle size of the ceramic powder is too small, the powder inertia is low, and the adhesion between powders is poor, so the formed ceramic coating is prone to powder shedding, which affects the appearance and corrosion resistance of the ceramic coating. On the other hand, the mechanism of ceramic coating formation is: using a single powder particle as a deposition unit, the sprayed powder particles collide with the substrate and the deposited coating at high speed, plastic deformation of the powder particles occurs, and due to the strong impact of the particles, an amorphous structure is formed locally in the coating. When the particle size is too small, powder agglomeration is likely to occur, making it difficult for the powder to be sprayed out of the spray gun. Or, due to the uneven particle size after powder agglomeration, the impact force of the particles in the powder impact process after spraying is uneven, which may cause uneven bonding between the ceramic coating and the substrate surface, seriously affecting the salt spray resistance of the coating. If the particle size is greater than 300nm, the pores between the ceramic powders are too large, the density of the film layer is poor, and the anti-corrosion performance of the coating cannot be guaranteed. In addition, the bonding between the formed ceramic film layer and the substrate is relatively poor.
[0023] Preferably, the time for grinding and chamfering in step (1) is 4-10 hours, for example, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, etc.
[0024] Preferably, the abrasive used for the chamfering in step (1) includes any one of triangular abrasives, trapezoidal abrasives, and circular abrasives, or a combination of at least two of them.
[0025] Preferably, the blasting medium used in the blasting in step (1) comprises corundum (such as brown corundum, etc.) and / or glass beads.
[0026] Preferably, the particle size of the sandblasting medium is 80-200 mesh, for example, 80 mesh, 90 mesh, 100 mesh, 120 mesh, 140 mesh, 160 mesh, 180 mesh, 200 mesh, etc.
[0027] Preferably, the pressure of the sandblasting process in step (1) is 0.1-1 MPa, for example, 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.5 MPa, 0.6 MPa, 0.8 MPa, 1 MPa, etc.
[0028] Preferably, during the sandblasting process of step (1), the distance between the spray gun and the NdFeB substrate is 100-150 mm, for example, 100 mm, 110 mm, 120 mm, 130 mm, 140 mm, 150 mm, etc.
[0029] Preferably, the sandblasting time in step (1) is 10-20 min, for example, 10 min, 12 min, 15 min, 18 min, 20 min, etc.
[0030] Preferably, the pickling time in step (1) is 10-120 s, for example, 10 s, 20 s, 30 s, 50 s, 80 s, 100 s, 120 s, etc.
[0031] Preferably, the pickling solution used in the pickling in step (1) comprises any one of hydrochloric acid, nitric acid and sulfuric acid, or a combination of at least two of them.
[0032] In the present invention, the purpose of pickling is to clean impurities such as dust and oil stains on the surface of the substrate.
[0033] Preferably, the ceramic powder in step (2) comprises any one of yttrium oxide, aluminum oxide, silicon oxide, aluminum nitride, silicon nitride, and zirconium oxide, or a combination of at least two thereof.
[0034] Preferably, the accelerated deposition rate of the ceramic powder in step (2) is 400-1000 m / s, such as 400 m / s, 500 m / s, 600 m / s, 700 m / s, 800 m / s, 900 m / s, 1000 m / s, etc. The present invention utilizes the impact energy generated by the high-speed expansion of ceramic powder particles at room temperature to continuously accumulate on the surface of the NdFeB substrate to form a ceramic coating.
[0035] Preferably, the pressure at the inlet of the spray gun for vacuum room temperature spraying in step (2) is 0.5-3 MPa, for example, 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, etc.
[0036] Preferably, the vacuum degree of the vacuum room temperature spraying in step (2) is 50-2000Pa, for example, 50Pa, 100Pa, 200Pa, 300Pa, 500Pa, 800Pa, 1000Pa, 1200Pa, 1400Pa, 1600Pa, 1800Pa, 2000Pa, etc.
[0037] Preferably, the working gas for the vacuum room temperature spraying in step (2) is an inert gas, including any one of nitrogen, argon, and helium, or a combination of at least two of them.
[0038] Preferably, the gas consumption flow rate of the vacuum room temperature spraying in step (2) is 3.5-8.5 L / min, for example, 3.5 L / min, 4 L / min, 5 L / min, 6 L / min, 7 L / min, 8 L / min, 8.5 L / min, etc.
[0039] Preferably, the spraying distance of the vacuum room temperature spraying in step (2) (i.e. the distance between the nozzle and the surface of the NdFeB substrate) is 10-30 mm, for example, 10 mm, 13 mm, 15 mm, 18 mm, 20 mm, 23 mm, 25 mm, 28 mm, 30 mm, etc.
[0040] Preferably, the scanning speed of the vacuum room temperature spraying in step (2) is 50-80 m / s, for example, 50 m / s, 52 m / s, 54 m / s, 56 m / s, 58 m / s, 60 m / s, 62 m / s, 64 m / s, 66 m / s, 68 m / s, 70 m / s, 72 m / s, 74 m / s, 76 m / s, 78 m / s, 80 m / s, etc.
[0041] As a preferred technical solution of the present invention, the scanning speed of the vacuum room temperature spraying in step (2) is divided into two stages, the scanning speed of the first stage is recorded as V1, and the scanning speed of the second stage is recorded as V2, V2 is 60%-85% of V1 (for example, 60%, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 85%, etc.), and when the film thickness reaches 80%-95% of the preset film thickness (for example, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 93%, 95%, etc.), the scanning speed of the spray gun is reduced to enter the second stage.
[0042] As a preferred technical solution of the present invention, the scanning speed of the vacuum room temperature spraying in step (2) is divided into two stages. The scanning speed of the first stage is 70-80m / s (for example, 70m / s, 72m / s, 74m / s, 76m / s, 78m / s, 80m / s, etc.). When the film thickness reaches 80%-95% (for example, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 93%, 95%, etc.) of the preset film thickness, the scanning speed of the spray gun is reduced to enter the second stage. The scanning speed of the second stage is 50-60m / s, for example, 50m / s, 52m / s, 54m / s, 56m / s, 58m / s, 60m / s, etc. Dividing the scanning speed into two stages has the following advantages while ensuring the film-forming efficiency: on the one hand, it can improve the flatness of the ceramic film surface; on the other hand, it can ensure that the thickness of the film at the corners of the NdFeB substrate is consistent with that of the film on the large surface, improve the bonding strength between the film at the corners and the substrate, improve the overall uniformity of the film on the substrate surface, and improve the corrosion resistance of the ceramic film, especially the corrosion resistance of the ceramic film under more extreme conditions such as high temperature and high pressure.
[0043] Preferably, the number of vacuum room temperature spraying in step (2) is 10-30 times / surface, for example, 10 times / surface, 12 times / surface, 14 times / surface, 16 times / surface, 18 times / surface, 20 times / surface, 22 times / surface, 24 times / surface, 26 times / surface, 28 times / surface, 30 times / surface, etc.
[0044] The ceramic coating prepared by the preparation method provided by the present invention has high hardness, good insulation, good bonding strength with the NdFeB substrate, good surface flatness, and good corrosion resistance; and the preparation process is simple and the production efficiency is high.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] (1) The ceramic coating for corrosion protection of NdFeB devices provided by the present invention has a layered stacked microstructure. The existence of this structure enables the coating to have both good overall uniformity and good corrosion resistance.
[0047] (2) The present invention is the first in the field of NdFeB to use a vacuum room temperature spraying process to form a ceramic coating. In the process of forming the coating, the substrate is sandblasted and the surface roughness after sandblasting is limited, and the particle size of the ceramic powder is controlled within a specific range. This improves the bonding strength between the coating and the substrate, improves the overall uniformity of the coating, and improves the corrosion resistance of the corners of the substrate, thereby ensuring the overall corrosion resistance of the NdFeB magnet. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1This is a cross-sectional SEM image of the ceramic coating for corrosion protection of NdFeB devices provided in Example 3 (magnification is 2000 times).
[0049] Figure 2 This is a cross-sectional SEM image of the ceramic coating for corrosion protection of NdFeB devices provided in Example 3 (magnification is 5000 times).
[0050] Figure 3 This is a cross-sectional SEM image of the whole formed by the ceramic coating and the NdFeB substrate provided in Example 3. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0052] Example 1
[0053] In this embodiment, a ceramic coating for corrosion protection of NdFeB devices is provided, and a preparation method thereof comprises the following steps:
[0054] (1) Matrix pretreatment: grinding, chamfering, sandblasting and pickling of the NdFeB matrix (NdFeB block magnet with specifications of 17.17*15.6*6.78 (mm));
[0055] Among them, the chamfering time is 8h, and the abrasive used for chamfering is round abrasive; the blasting medium used for sandblasting is brown corundum with a particle size of 180 mesh, the pressure of the sandblasting process is 0.1MPa, the distance between the spray gun and the NdFeB substrate is 100mm, and the sandblasting time is 10min; the pickling time is 30s, the pickling liquid is dilute nitric acid, and the surface roughness of the NdFeB substrate obtained after pickling is 2.56μm.
[0056] (2) Vacuum room temperature spraying: using a vacuum room temperature spraying method to deposit ceramic powder on the surface of the NdFeB substrate after pickling obtained in step (1), to obtain the ceramic coating for corrosion protection of NdFeB devices;
[0057] Among them, the ceramic powder is Al2O3 powder with a particle size of 300nm; the deposition speed of the ceramic powder after acceleration is 470m / s; the pressure at the inlet of the spray gun for vacuum room temperature spraying is 1MPa, the vacuum degree is 100Pa, the working gas is inert gas argon, the gas flow rate is 5L / min, the gas temperature is 200℃, the distance between the nozzle and the surface of the iron boron substrate is 30mm, and the scanning speed of the nozzle is divided into two stages. The scanning speed of the first stage is 80m / s. When the film thickness is 8μm away from the preset film thickness, the scanning speed of the spray gun is reduced to enter the second stage. The scanning speed of the second stage is 50m / s; the number of spraying is 20 times / surface.
[0058] Example 2
[0059] In this embodiment, a ceramic coating for corrosion protection of NdFeB devices is provided, and a preparation method thereof comprises the following steps:
[0060] (1) Matrix pretreatment: grinding, chamfering, sandblasting and pickling of the NdFeB matrix (NdFeB block magnet with specifications of 17.17*15.6*6.78 (mm));
[0061] Among them, the chamfering time is 10h, and the abrasive used for chamfering is round abrasive; the blasting medium used for sandblasting is glass beads with a particle size of 180 mesh, the pressure of the sandblasting process is 0.1MPa, the distance between the spray gun and the NdFeB substrate is 100mm, and the sandblasting time is 20min; the pickling time is 30s, the pickling liquid is dilute nitric acid, and the surface roughness of the NdFeB substrate obtained after pickling is 2.74μm.
[0062] (2) Vacuum room temperature spraying: using a vacuum room temperature spraying method to deposit ceramic powder on the surface of the NdFeB substrate after pickling obtained in step (1), to obtain the ceramic coating for corrosion protection of NdFeB devices;
[0063] Among them, the ceramic powder is Y2O3 powder with a particle size of 200nm; the deposition speed of the ceramic powder after acceleration is 545m / s; the pressure at the inlet of the spray gun for vacuum room temperature spraying is 2MPa, the vacuum degree is 100Pa, the working gas is inert gas argon, the gas flow rate is 5L / min, the gas temperature is 200℃, the distance between the nozzle and the surface of the iron boron substrate is 10mm, and the scanning speed of the nozzle is divided into two stages. The scanning speed of the first stage is 80m / s. When the film thickness is 10μm away from the preset film thickness, the scanning speed of the spray gun is reduced to enter the second stage. The scanning speed of the second stage is 50m / s; the number of spraying is 20 times / surface.
[0064] Example 3
[0065] In this embodiment, a ceramic coating for corrosion protection of NdFeB devices is provided, and a preparation method thereof comprises the following steps:
[0066] (1) Matrix pretreatment: grinding, chamfering, sandblasting and pickling of the NdFeB matrix (NdFeB block magnet with specifications of 17.17*15.6*6.78 (mm));
[0067] Among them, the chamfering time is 6h, and the abrasive used for chamfering is triangular abrasive; the blasting medium used for sandblasting is brown corundum with a particle size of 180 mesh. The pressure of the sandblasting process is 0.5MPa, the distance between the spray gun and the NdFeB substrate is 100mm, and the sandblasting time is 10min; the pickling time is 30s, the pickling liquid is dilute nitric acid, and the surface roughness of the NdFeB substrate obtained after pickling is 2.26μm.
[0068] (2) Vacuum room temperature spraying: using a vacuum room temperature spraying method to deposit ceramic powder on the surface of the NdFeB substrate after pickling obtained in step (1), to obtain the ceramic coating for corrosion protection of NdFeB devices;
[0069] Among them, the ceramic powder is Al2O3 powder with a particle size of 300nm; the deposition speed of the ceramic powder after acceleration is 565m / s; the pressure at the inlet of the spray gun for vacuum room temperature spraying is 2.5MPa, the vacuum degree is 100Pa, the working gas is inert gas argon, the gas flow rate is 5L / min, the gas temperature is 200℃, the distance between the nozzle and the surface of the iron boron substrate is 10mm, and the scanning speed of the nozzle is divided into two stages. The scanning speed of the first stage is 80m / s. When the film thickness is 10μm away from the preset film thickness, the scanning speed of the spray gun is reduced to enter the second stage. The scanning speed of the second stage is 60m / s; the number of spraying is 30 times / surface.
[0070] The cross-sectional SEM image of the ceramic coating for corrosion protection of NdFeB devices provided in this embodiment is as follows: Figure 1 and Figure 2 As shown, Figure 1 The magnification is 2000 times. Figure 2 The magnification is 5000 times, and it can be seen that the ceramic coating has a layered stacked microstructure.
[0071] The cross-sectional SEM image of the whole formed by the ceramic coating and the NdFeB substrate provided in this embodiment is as follows: Figure 3 As shown, it can be seen that the ceramic coating is tightly bonded to the NdFeB substrate.
[0072] Example 4
[0073] In this embodiment, a ceramic coating for corrosion protection of NdFeB devices is provided, and a preparation method thereof comprises the following steps:
[0074] (1) Matrix pretreatment: grinding, chamfering, sandblasting and pickling of the NdFeB matrix (NdFeB block magnet with specifications of 17.17*15.6*6.78 (mm));
[0075] Among them, the chamfering time is 4h, and the abrasive used for chamfering is round abrasive; the blasting medium used for sandblasting is brown corundum with a particle size of 80 mesh, the pressure of the sandblasting process is 0.1MPa, the distance between the spray gun and the NdFeB substrate is 100mm, and the sandblasting time is 10min; the pickling time is 30s, and the pickling solution is a mixture of dilute nitric acid and dilute sulfuric acid (the volume ratio of the two is 1:1). The surface roughness of the NdFeB substrate obtained after pickling is 1.4μm.
[0076] (2) Vacuum room temperature spraying: using a vacuum room temperature spraying method to deposit ceramic powder on the surface of the NdFeB substrate after pickling obtained in step (1), to obtain the ceramic coating for corrosion protection of NdFeB devices;
[0077] Among them, the ceramic powder is aluminum nitride powder with a particle size of 250nm; the deposition speed of the ceramic powder after acceleration is 500m / s; the pressure at the inlet of the spray gun for vacuum room temperature spraying is 0.5MPa, the vacuum degree is 100Pa, the working gas is inert gas argon, the gas flow rate is 6L / min, the gas temperature is 200℃, the distance between the nozzle and the surface of the iron boron substrate is 25mm, and the scanning speed of the nozzle is divided into two stages. The scanning speed of the first stage is 70m / s. When the film thickness is 12μm away from the preset film thickness, the scanning speed of the spray gun is reduced to enter the second stage. The scanning speed of the second stage is 50m / s; the number of spraying is 20 times / surface.
[0078] Example 5
[0079] The only difference between this embodiment and embodiment 1 is that the scanning speed of the nozzle in step (2) is not carried out in stages, and the specific scanning speed is 80 m / s.
[0080] Comparative Example 1
[0081] The only difference between this comparative example and Example 1 is that the conditions of the sandblasting process in step (1) are different, specifically: the sandblasting medium used for sandblasting is brown corundum with a particle size of 200 mesh, the pressure of the sandblasting process is 1.2 MPa, the distance between the spray gun and the NdFeB substrate is 100 mm, and the sandblasting time is 8 min; ultimately, the surface roughness of the NdFeB substrate obtained after the pickling is 1 μm.
[0082] Comparative Example 2
[0083] The only difference between this comparative example and Example 1 is that the conditions of the sandblasting process in step (1) are different, specifically: the sandblasting medium used for sandblasting is brown corundum with a particle size of 60 mesh, the pressure of the sandblasting process is 0.08 MPa, the distance between the spray gun and the NdFeB substrate is 100 mm, and the sandblasting time is 30 min; ultimately, the surface roughness of the NdFeB substrate obtained after the pickling is 3.1 μm.
[0084] Comparative Example 3
[0085] The only difference between this comparative example and Example 1 is that the particle size of the Al2O3 powder used in step (2) is 50 nm.
[0086] Comparative Example 4
[0087] The only difference between this comparative example and Example 1 is that the particle size of the Al2O3 powder used in step (2) is 350nm.
[0088] The ceramic coatings provided in the embodiments and comparative examples were subjected to performance tests, wherein the surface roughness of the ceramic coatings, the neutral salt spray resistance test duration, the moisture and heat resistance test duration, and the bonding strength between the ceramic coatings and the surface of the NdFeB substrate are as described in the above content of the invention and will not be repeated here.
[0089] The performance test results are shown in Table 1.
[0090] Table 1
[0091]
[0092]
[0093] It can be seen from Table 1 that the ceramic coatings provided in the embodiments of the present invention have good corrosion resistance (neutral salt spray resistance test duration: 348-1032h; moisture and heat resistance test duration: 96-324h), and have good bonding strength with the NdFeB substrate (22.43-26.49MPa) and good surface flatness (surface roughness: 2.15-3.1μm).
[0094] Compared with Example 1, the bonding strength between the ceramic coating provided in Comparative Example 1 and the surface of the NdFeB substrate is significantly worse, and the duration of the moisture and heat resistance test is significantly shortened; the surface flatness of the ceramic coating provided in Comparative Example 2 is worse, and the corrosion resistance is worse; the corrosion resistance of the ceramic coating provided in Comparative Example 3 is significantly worse, and the bonding strength between the ceramic coating and the surface of the NdFeB substrate is significantly worse; the corrosion resistance of the ceramic coating provided in Comparative Example 4 is significantly worse, and the bonding strength between the ceramic coating and the surface of the NdFeB substrate is worse.
[0095] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the ceramic coating for corrosion protection of NdFeB devices and the preparation method thereof, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A ceramic coating for corrosion protection of NdFeB devices, characterized in that: Scanning electron microscopy was used for characterization, and when the magnification was 1000-7000 times, it was observed that the ceramic coating had a layered stacked microstructure.
2. The ceramic coating for corrosion protection of NdFeB devices according to claim 1, characterized in that: The composition of the ceramic coating includes any one or a combination of at least two of yttrium oxide, aluminum oxide, silicon oxide, aluminum nitride, silicon nitride, and zirconium oxide; Preferably, the ceramic coating has a thickness of 20-200 μm.
3. The ceramic coating for corrosion protection of NdFeB devices according to claim 1 or 2, characterized in that: The surface roughness of the ceramic coating is 2.1-3.2 μm; Preferably, the neutral salt spray resistance test duration of the ceramic coating is ≥ 340 h; Preferably, the moisture and heat resistance test duration of the ceramic coating is ≥ 192h; Preferably, the bonding force between the ceramic coating and the surface of the NdFeB substrate is ≥20 MPa.
4. A method for preparing a ceramic coating for corrosion protection of NdFeB devices as claimed in any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) Matrix pretreatment: grinding, chamfering, sandblasting and pickling of the NdFeB matrix; (2) Vacuum room temperature spraying: using a vacuum room temperature spraying method to deposit ceramic powder on the surface of the NdFeB substrate after pickling obtained in step (1), to obtain the ceramic coating for corrosion protection of NdFeB devices; The surface roughness of the NdFeB substrate obtained after step (1) is 1.3-3.0 μm; The particle size of the ceramic powder in step (2) is 100-300nm.
5. The preparation method according to claim 4, characterized in that: The time for grinding and chamfering in step (1) is 4-10 hours; Preferably, the abrasive used for the chamfering in step (1) includes any one of triangular abrasives, trapezoidal abrasives, and circular abrasives, or a combination of at least two of them.
6. The preparation method according to claim 4 or 5, characterized in that: The sandblasting medium used in the sandblasting of step (1) includes corundum and / or glass beads; Preferably, the particle size of the sandblasting medium is 80-200 mesh.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The pressure of the sandblasting process in step (1) is 0.1-1 MPa; Preferably, during the sandblasting process in step (1), the distance between the spray gun and the NdFeB substrate is 100-150 mm; Preferably, the sandblasting time in step (1) is 10-20 minutes.
8. The preparation method according to any one of claims 4 to 7, characterized in that: The pickling time in step (1) is 10-120s; Preferably, the pickling solution used for pickling in step (1) comprises any one of hydrochloric acid, nitric acid and sulfuric acid, or a combination of at least two of them.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The ceramic powder in step (2) comprises any one of yttrium oxide, aluminum oxide, silicon oxide, aluminum nitride, silicon nitride, and zirconium oxide, or a combination of at least two thereof; Preferably, the accelerated deposition rate of the ceramic powder in step (2) is 400-1000 m / s.
10. The preparation method according to any one of claims 4 to 9, characterized in that: The pressure at the inlet of the spray gun for vacuum room temperature spraying in step (2) is 0.5-3MPa; Preferably, the vacuum degree of the vacuum spraying at room temperature in step (2) is 50-2000 Pa; Preferably, the working gas for vacuum room temperature spraying in step (2) is an inert gas, including any one of nitrogen, argon, and helium, or a combination of at least two of them; Preferably, the gas consumption flow rate of the vacuum room temperature spraying in step (2) is 3.5-8.5 L / min; Preferably, the spraying distance of the vacuum room temperature spraying in step (2) is 10-30 mm; Preferably, the scanning speed of the vacuum room temperature spraying in step (2) is 50-80 m / s; Preferably, the scanning speed of the vacuum room temperature spraying in step (2) is divided into two stages, the scanning speed of the first stage is recorded as V1, and the scanning speed of the second stage is recorded as V2, V2 is 60%-85% of V1, and when the film thickness reaches 80%-95% of the preset film thickness, the scanning speed of the spray gun is reduced to enter the second stage; Preferably, the scanning speed of the vacuum room temperature spraying in step (2) is divided into two stages, the scanning speed of the first stage is 70-80 m / s, when the film thickness reaches 80%-95% of the preset film thickness, the scanning speed of the spray gun is reduced to enter the second stage, the scanning speed of the second stage is 50-60 m / s; Preferably, the vacuum room temperature spraying in step (2) is performed 10-30 times per surface.