Method for preparing nickel-based coating on surface of copper alloy through high-speed laser cladding
Through high-speed laser cladding technology, the use of coaxial powder feeding on the surface of copper alloy is used to form a micro-melting pool, which solves the quality and efficiency problems in the preparation of nickel-based coating on the surface of copper alloy, and achieves efficient and dense coating preparation and performance improvement.
Patent Information
- Application Number
- CN202410546091.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art When preparing nickel-based coatings on laser cladding on copper alloy surfaces, there are problems such as uncontrollable coating quality, complex process and low efficiency, especially due to the large laser reflectivity and large heat input, resulting in poor internal quality of the coating. and low preparation efficiency.
Using high-speed laser cladding method, a micro-melting pool is formed on the surface of copper alloy by coaxial powder feeding, controlling laser power and scanning speed, simplifying the process, improving preparation efficiency, promoting metallurgical bonding and interface diffusion, and ensuring coating quality and bonding strength.
The high-quality preparation of nickel-based coatings is achieved, the process flow is simplified, the preparation efficiency is improved, the dense bonding and high bonding strength between the coating and the substrate is ensured, and the coating performance is improved.
Smart Images

Figure CN119061394A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal coating preparation, and relates to a method for preparing a nickel-based coating by high-speed laser cladding on the surface of a copper alloy. Background Art
[0002] Copper and copper alloys are an important type of metal material with excellent electrical and thermal conductivity, corrosion resistance, fatigue resistance and other properties. They are widely used in electrical, electronic, mobile communications, new energy vehicles, aerospace, rail transit and other fields. However, due to the low hardness, poor wear resistance and poor ablation resistance of copper alloys, surface wear and ablation have become one of the main causes of failure of copper alloy components. Therefore, there is an urgent need to improve the surface properties of copper alloys to extend the service life of components.
[0003] To improve the surface performance of copper alloys, preparing a coating on its surface is one of the common ways to improve the corresponding performance. Among the methods for preparing coatings, laser cladding has great advantages because the prepared coating has a dense structure, high bonding strength, and excellent performance, especially for the preparation of metal coatings. Based on the characteristics of copper alloys, the material of the coating needs to be selected with a material that has high solubility with copper metal and small physical property differences, such as nickel-based alloys, which not only meet the requirements of mutual solubility, but also have high hardness, good wear resistance, high temperature resistance and other properties to make up for the defects of the copper alloy's own performance. Since copper alloys have high laser reflectivity and thermal conductivity, it is difficult for laser energy to form a molten pool on the surface of copper alloys when using laser cladding technology. Therefore, conventional laser cladding technology requires the use of pre-set powders, laser remelting and other methods to prepare nickel-based coatings, but there are disadvantages such as difficult to control the internal quality of the coating, large heat input, complex process, and low efficiency.
[0004] CN 116555757A discloses a method for reducing reflectivity during laser cladding of a copper alloy substrate, the method comprising: roughening the surface of a copper alloy workpiece, then brushing a volatile glue on the target surface, then spreading nickel-based alloy powder on the target surface to completely cover the target surface, shaking off the unattached nickel-based alloy powder and drying to form a transition layer, and preparing a target coating on the transition layer. The method adopts the traditional method of laying powder before laser cladding, which has many preparation processes, slow cladding speed, and long preparation time, greatly reducing the preparation efficiency; the requirements for brushing volatile glue, spreading powder and drying are high, which easily affects the uniformity of the coating, and the volatile glue easily causes defects such as pores in the coating, thereby leading to problems such as a narrow preparation process window and poor internal quality of the nickel-based alloy coating.
[0005] High-speed laser cladding technology uses laser energy to melt the powder above the substrate, and then solidifies with the micro-molten pool on the surface of the substrate to form a coating, which changes the forming method of the coating and can solve the problem of difficulty in forming a large-sized molten pool on the surface of the substrate to a certain extent. CN 116083914A discloses a method for laser cladding of self-fluxing nickel-based alloy powder on a copper alloy glass mold, the method comprising: rough processing before laser cladding; pre-stress relief annealing; shot blasting, the cladding area of the semi-finished copper alloy glass mold after stress relief annealing is shot blasted; preheating before laser cladding, placing the semi-finished product in a heating furnace for preheating; laser cladding, according to the cladding motion trajectory program, the nickel-based alloy powder is clad to the cladding area through the laser cladding process; stress relief annealing after laser cladding to obtain the copper alloy glass mold. The method has many operating steps, including preheating, two stress annealings and shot blasting, a long preparation process, an incomplete introduction to the cladding process, and no clear parameters such as its scanning rate.
[0006] In summary, in order to solve the problems of high laser reflectivity on the copper alloy surface and large heat input in the cladding process, the pre-set powder method was used to increase the laser absorptivity, and the preheating-stress relief annealing method was used to reduce stress and strain to achieve the preparation of nickel-based coating on the copper alloy surface. However, there are still problems such as uncontrollable coating quality, complicated process and low efficiency. Summary of the invention
[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing a nickel-based coating on the surface of a copper alloy by high-speed laser cladding. The high-speed laser cladding method adopts a coaxial powder feeding method to prepare the nickel-based coating, and the powder melts in the air, which can significantly improve the preparation efficiency; only a micro-molten pool needs to be formed on the surface of the copper alloy to promote the diffusion of elements between the coating and the substrate to form a metallurgical bond, thereby ensuring the interface bonding density and high bonding strength between the coating and the substrate, and at the same time having little thermal impact on the copper alloy substrate.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] The present invention provides a method for preparing a nickel-based coating on a copper alloy surface by high-speed laser cladding, the method comprising the following steps:
[0010] (1) sandblasting the surface of the copper alloy, and then cleaning it to obtain a pretreated copper alloy substrate;
[0011] (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the high-speed laser cladding adopts a coaxial powder feeding method, the laser power is 2500-3500 W, and the laser scanning speed is 4.8-9 m / min to prepare a nickel-based coating; wherein the laser power can be selected from 2500 W, 2600 W, 2700 W, 2800 W, 3000 W, 3200 W, 3400 W or 3500 W, etc., and the laser scanning speed can be selected from 4.8 m / min, 5 m / min, 5.5 m / min, 6 m / min, 6.5 m / min, 7 m / min, 7.5 m / min, 8 m / min or 9 m / min, etc., but are not limited to the listed values, and other values not listed within the respective numerical ranges are also applicable.
[0012] In the present invention, a high-speed laser cladding method is adopted for the preparation of a nickel-based coating on the surface of a copper alloy substrate, specifically a coaxial powder feeding method is adopted, and there is no need to adopt a prefabricated powder method, which can greatly simplify the process, shorten the preparation time, and improve the preparation efficiency. Only a micro-molten pool is formed on the surface of the substrate, and the required laser energy is small, and the thermal impact on the copper alloy is also small; by controlling the high-speed laser cladding process parameters, such as laser power, scanning speed, working distance, etc., the heat input of the laser is controlled, the powder is fully melted, and the internal quality of the coating is high and defect-free, and the diffusion of interface elements in the coating forming process is promoted through the formation of a surface micro-molten pool, which is beneficial to the formation of metallurgical bonding and ensures the dense bonding and high bonding strength between the coating and the substrate; the higher scanning speed makes the cooling rate of the coating higher after laser cladding, which can promote the refinement of the internal structure of the coating and further improve the coating performance; the method has a simple process flow, is easy to operate, has a low cost, and has a wider range of applications.
[0013] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0014] As a preferred technical solution of the present invention, the copper alloy in step (1) includes any one of oxide dispersion strengthened copper, zirconium copper alloy or nickel copper alloy, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of oxide dispersion strengthened copper and zirconium copper alloy, a combination of zirconium copper alloy and nickel copper alloy, a combination of oxide dispersion strengthened copper, zirconium copper alloy and nickel copper alloy, etc.
[0015] In the present invention, according to the specific application of the copper alloy, the copper alloy is generally selected to have high strength and high electrical conductivity.
[0016] Preferably, the copper alloy in step (1) is used as a component of a continuous casting crystallizer, a blast furnace tuyere or an electrical contact.
[0017] As a preferred technical solution of the present invention, the sandblasting treatment in step (1) is to use sand particles to spray the surface of the copper alloy.
[0018] Preferably, the sand particles include any one of aluminum oxide particles, glass sand, silicon carbide particles or silicon nitride particles, or a combination of at least two of them. Typical but non-limiting examples of the combinations include: a combination of aluminum oxide particles and glass sand, a combination of glass sand and silicon nitride particles, a combination of silicon carbide particles and silicon nitride particles, a combination of aluminum oxide particles, glass sand and silicon nitride particles, a combination of aluminum oxide particles, silicon carbide particles and silicon nitride particles, and the like.
[0019] Preferably, the particle size of the sand particles is 80-200 mesh, for example 80 mesh, 100 mesh, 125 mesh, 140 mesh, 160 mesh, 180 mesh or 200 mesh, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the spray angle of the sandblasting in step (1) is 30 to 60 degrees, for example, 30 degrees, 35 degrees, 40 degrees, 45 degrees, 50 degrees, 55 degrees or 60 degrees, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the spray pressure of the sandblasting treatment in step (1) is 0.3-0.5 MPa, for example 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa, 0.5 MPa, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the sandblasting in step (1) is stopped until the surface of the copper alloy is rough without obvious reflective or bright areas, and the surface roughness at this time is 10 to 20 μm, for example, 10 μm, 12 μm, 14 μm, 15 μm, 16 μm, 18 μm or 20 μm, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] In the present invention, the sandblasting treatment can achieve the purpose of activating the substrate surface, increasing the surface roughness and reducing the laser reflectivity, thereby facilitating the formation of a molten pool on the substrate surface.
[0024] As a preferred technical solution of the present invention, the cleaning method in step (1) includes ultrasonic cleaning.
[0025] Preferably, an organic solvent is used as a cleaning medium during the ultrasonic cleaning.
[0026] Preferably, the organic solvent comprises ethanol and / or acetone.
[0027] Preferably, the power of the ultrasonic cleaning is 25-50 W, for example, 25 W, 30 W, 35 W, 40 W, 45 W or 50 W, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] Preferably, the ultrasonic cleaning time is 5 to 10 minutes, for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] As a preferred technical solution of the present invention, the raw material used in the high-speed laser cladding in step (2) includes nickel-based powder.
[0030] Preferably, the nickel-based powder is an aluminum-coated nickel core-shell structure powder or a mixed powder of nickel powder and aluminum powder.
[0031] Preferably, the mass fraction of nickel in the nickel-based powder is 85-95wt%, for example 85wt%, 86wt%, 88wt%, 90wt%, 92wt%, 94wt% or 95wt%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the particle size of the nickel-based powder is 53-106 μm, for example, 53 μm, 63 μm, 74 μm, 88 μm, 95 μm, 100 μm or 106 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] As a preferred technical solution of the present invention, the high-speed laser cladding in step (2) is carried out using a high-speed laser cladding equipment, and the standard mobile laser cladding equipment of Huirui can be selected.
[0034] Preferably, the laser cladding head of the high-speed laser cladding equipment uses an annular coaxial powder feeding nozzle for powder delivery.
[0035] Preferably, during the high-speed laser cladding, the distance between the end of the laser cladding head and the surface of the copper alloy substrate is 20 to 22 mm, for example, 20 mm, 20.5 mm, 21 mm, 21.5 mm or 22 mm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] As a preferred technical solution of the present invention, the laser spot diameter during the high-speed laser cladding in step (2) is 2 to 2.5 mm, for example, 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm or 2.5 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the scanning path of the laser is a reciprocating movement along an S-shape.
[0038] Preferably, the overlap rate between single tracks during laser scanning is 60-80%, for example 60%, 63%, 65%, 68%, 70%, 72%, 75%, 78% or 80%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] In the present invention, the overlap rate refers to the ratio of overlap between two adjacent scanning paths. Due to the fast scanning speed, one scan may not be able to meet the requirements. Selecting a higher overlap rate allows the same position to be scanned several times to ensure the formation of a surface micro-molten pool, which also helps to evenly distribute the molten powder on the surface.
[0040] As a preferred technical solution of the present invention, the powder feeding flow rate during the high-speed laser cladding in step (2) is 4.6 to 7.8 g / min, for example, 4.6 g / min, 5.0 g / min, 5.5 g / min, 6.0 g / min, 6.5 g / min, 7.0 g / min, 7.5 g / min or 7.8 g / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, the nickel-based powder is mixed with a powder feeding gas and then sprayed out, and the flow rate of the powder feeding gas is 7 to 12 L / min, for example, 7 L / min, 8 L / min, 9 L / min, 10 L / min, 11 L / min or 12 L / min, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] Preferably, a protective gas is introduced during the high-speed laser cladding, and the flow rate of the protective gas is 10 to 15 L / min, for example, 10 L / min, 11 L / min, 12 L / min, 13 L / min, 14 L / min or 15 L / min, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0043] Preferably, the powder feeding gas is ejected from a powder feeding port of a nozzle of the laser cladding head, and the shielding gas is ejected from the middle of the nozzle of the laser cladding head.
[0044] Preferably, the powder feeding gas and the protective gas independently include inert gas and / or nitrogen, and the inert gas includes argon, neon or helium.
[0045] As a preferred technical solution of the present invention, after the high-speed laser cladding in step (2) is completed, it is placed in the air for natural cooling.
[0046] Preferably, the thickness of the nickel-based coating in step (2) is 400 to 600 μm, for example, 400 μm, 450 μm, 500 μm, 550 μm or 600 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] As a preferred technical solution of the present invention, the method comprises the following steps:
[0048] (1) sandblasting the surface of the copper alloy, wherein the sandblasting is performed by spraying the surface of the copper alloy with sand particles, wherein the sand particles include any one of aluminum oxide particles, glass sand, silicon carbide particles, or silicon nitride particles, or a combination of at least two of the particles, wherein the particle size of the sand particles is 80 to 200 meshes, the spraying angle of the sandblasting is 30 to 60 degrees, and the spraying pressure is 0.3 to 0.5 MPa. The sandblasting is stopped after the surface roughness of the copper alloy reaches 10 to 20 μm, and then ultrasonic cleaning is performed, wherein an organic solvent is used as a cleaning medium, the power of the ultrasonic cleaning is 25 to 50 W, and the time is 5 to 10 min, to obtain a pretreated copper alloy substrate;
[0049] (2) high-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the raw materials used for the high-speed laser cladding include nickel-based powder, wherein the nickel-based powder is a core-shell structure powder of aluminum-coated nickel or a mixed powder of nickel powder and aluminum powder, wherein the mass fraction of nickel in the nickel-based powder is 85-95wt%, and the particle size is 53-106μm, and the nickel-based powder is sprayed by coaxial powder feeding. The laser power during the high-speed laser cladding is 2500-3500W, the laser scanning speed is 4.8-9m / min, and the working distance is 20-22mm. The laser spot diameter is 2-2.5 mm, the scanning path is to move back and forth along an S-shape, and the overlap rate is 60-80%; the powder feeding flow rate during the high-speed laser cladding is 4.6-7.8 g / min, the nickel-based powder is mixed with the powder feeding gas and then sprayed out, the flow rate of the powder feeding gas is 7-12 L / min, and the protective gas is introduced during the high-speed laser cladding, and the flow rate of the protective gas is 10-15 L / min. After the high-speed laser cladding is completed, it is placed in the air for natural cooling to obtain a nickel-based coating, and the thickness of the nickel-based coating is 400-600 μm.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] (1) The high-speed laser cladding method of the present invention adopts a coaxial powder feeding method to prepare a nickel-based coating, without the need for a prefabricated powder method, which can expand the application range of the processed substrate; the powder melts in the air, which can greatly increase the scanning speed and improve the preparation efficiency;
[0052] (2) During the preparation process, the method of the present invention only needs to form a micro-molten pool on the substrate, which solidifies with the molten powder to form a dense metallurgical bond. The required laser energy is small, the heat input and thermal impact on the substrate are small, and no preheating-annealing process and equipment are required, which can simplify the preparation process and improve the preparation efficiency.
[0053] (3) The method of the present invention has a simple process flow, is easy to operate, and has low cost. By controlling the process parameters, it can promote the full melting of the powder and the formation of a micro-molten pool on the surface of the substrate, achieve high-quality forming inside the coating and strong bonding with the substrate, and ensure that the coating has excellent performance; at the same time, the higher scanning speed accelerates the solidification cooling rate, which can promote the refinement of the internal structure of the coating and further improve the coating performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 is a schematic diagram of the cross-sectional morphology of the nickel-based coating provided in Example 1 of the present invention;
[0055] Figure 2 is a cross-sectional organizational structure diagram of the nickel-based coating provided in Example 1 of the present invention;
[0056] Figure 3 is an element distribution diagram of the interface between the copper alloy substrate and the nickel-based coating provided in Example 1 of the present invention;
[0057] Figure 4 is a microhardness result diagram of the copper alloy substrate and the nickel-based coating provided in Example 1 of the present invention;
[0058] Figure 5 This is a graph showing the arc ablation test results of the copper alloy substrate provided in Example 1 of the present invention;
[0059] Figure 6 This is a graph showing the arc ablation test results of the nickel-based coating provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0060] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0061] The specific implementation method of the present invention provides a method for preparing a nickel-based coating by high-speed laser cladding on a copper alloy surface, the method comprising the following steps:
[0062] (1) sandblasting the surface of the copper alloy, and then cleaning it to obtain a pretreated copper alloy substrate;
[0063] (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the high-speed laser cladding adopts a coaxial powder feeding method, a laser power of 2500 to 3500 W, and a laser scanning speed of 4.8 to 9 m / min to prepare a nickel-based coating.
[0064] The following are typical but non-limiting embodiments of the present invention:
[0065] Embodiment 1:
[0066] This embodiment provides a method for preparing a nickel-based coating by high-speed laser cladding on a copper alloy surface, the method comprising the following steps:
[0067] (1) sandblasting the copper alloy surface, wherein the sandblasting is performed by spraying the copper alloy surface with sand particles, wherein the sand particles are aluminum oxide particles, and the average particle size of the sand particles is 120 meshes, the spraying angle of the sandblasting is 45 degrees, and the spraying pressure is 0.5 MPa. The sandblasting is stopped after the surface roughness of the copper alloy reaches 15 μm, and then ultrasonic cleaning is performed, wherein anhydrous ethanol is used as the cleaning medium during the ultrasonic cleaning, and the power of the ultrasonic cleaning is 30 W, and the time is 5 min, to obtain a pretreated copper alloy substrate;
[0068] (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the raw material used for the high-speed laser cladding is nickel-based powder, the nickel-based powder is a core-shell structure powder of aluminum-coated nickel, the mass fraction of nickel in the nickel-based powder is 92wt%, and the average particle size is 74μm. The nickel-based powder is sprayed by coaxial powder feeding. The laser power during the high-speed laser cladding is 2700W, the laser scanning speed is 6m / min, the working distance is 21mm, the laser spot diameter is 2mm, the scanning path is an S-shaped reciprocating movement, and the overlap rate is 80%; the powder feeding flow rate during the high-speed laser cladding is 5.6g / min, the nickel-based powder is mixed with argon powder feeding gas and then sprayed, the flow rate of the powder feeding gas is 7L / min, and a protective gas is introduced during the high-speed laser cladding, the protective gas is argon, and its flow rate is 15L / min. After the high-speed laser cladding is completed, it is placed in the air for natural cooling to obtain a nickel-based coating, and the thickness of the nickel-based coating is 500μm.
[0069] In this embodiment, the nickel-based coating prepared on the copper alloy substrate is characterized by its cross-sectional morphology. Figure 1 Its cross-sectional structure is shown in Figure 2 As shown, the element distribution at the interface between the copper alloy substrate and the nickel-based coating was detected, and the results are shown in Figure 3 As shown;
[0070] The microhardness of the copper alloy substrate and the nickel-based coating was measured using a micro Vickers hardness tester (SHIMADZU, HMV-G-XY-S). Figure 4 As shown in FIG. 1 , the test conditions of the micro Vickers hardness tester are as follows: load 1.96 N, loading time 15 s; the conductivity of the copper alloy substrate and the nickel-based coating is measured on a QJ44 DC bridge using a four-point contact method; an arc ablation tester modified from a CSM-200 DC constant voltage pulse power supply is used to perform arc ablation tests on the copper alloy substrate and the nickel-based coating, and the results are shown in FIG. Figure 5 and Figure 6 shown.
[0071] In this embodiment, the nickel-based coating prepared by the above method is Figure 1 It can be seen that the surface of the nickel-based coating is flat, and the roughness is only 9.8 μm; Figure 2 It can be seen that the internal structure of the nickel-based coating is dense and has no obvious defects. Figure 3 It can be seen that the interface between the copper alloy substrate and the nickel-based coating presents an obvious metallurgical bond, and the diffusion distance can reach 77.8 μm;
[0072] Depend on Figure 4 It can be seen that the microhardness of the nickel-based coating is 191.7HV 0.2 Its hardness is 1.83 times that of the copper alloy substrate; according to the conductivity test results, the conductivity of the nickel-based coating is 18.03% IACS, which is close to that of pure nickel metal; Figure 5 and Figure 6 It can be seen that the nickel-based coating forms a volume of 2.16×10 7 μm 3 The ablation pit of the copper alloy substrate is reduced by 80.83%.
[0073] Embodiment 2:
[0074] This embodiment provides a method for preparing a nickel-based coating by high-speed laser cladding on a copper alloy surface, the method comprising the following steps:
[0075] (1) sandblasting the copper alloy surface, wherein the sandblasting is performed by spraying the copper alloy surface with sand particles, wherein the sand particles are aluminum oxide particles, and the average particle size of the sand particles is 150 meshes, the spraying angle of the sandblasting is 30 degrees, and the spraying pressure is 0.4 MPa. The sandblasting is stopped after the surface roughness of the copper alloy reaches 12 μm, and then ultrasonic cleaning is performed, wherein anhydrous ethanol is used as a cleaning medium during the ultrasonic cleaning, and the power of the ultrasonic cleaning is 35 W, and the time is 8 minutes, to obtain a pretreated copper alloy substrate;
[0076] (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the raw material used for the high-speed laser cladding is nickel-based powder, the nickel-based powder is a core-shell structure powder of aluminum-coated nickel, the mass fraction of nickel in the nickel-based powder is 90wt%, and the average particle size is 55μm. The nickel-based powder is sprayed by coaxial powder feeding. The laser power during the high-speed laser cladding is 3000W, the laser scanning speed is 7m / min, the working distance is 20mm, the laser spot diameter is 2.2mm, the scanning path is an S-shaped reciprocating movement, and the overlap rate is 70%; the powder feeding flow rate during the high-speed laser cladding is 6.5g / min, the nickel-based powder is mixed with argon powder feeding gas and then sprayed, the flow rate of the powder feeding gas is 10L / min, and a protective gas is introduced during the high-speed laser cladding, and the protective gas is argon gas with a flow rate of 12L / min. After the high-speed laser cladding is completed, it is placed in the air for natural cooling to obtain a nickel-based coating, and the thickness of the nickel-based coating is 400μm.
[0077] The test method of the nickel-based coating refers to the test method in Example 1.
[0078] In this embodiment, the nickel-based coating prepared by the above method has a smooth surface, a dense internal structure, and no obvious defects. The interface between the copper alloy substrate and the nickel-based coating is obviously metallurgically bonded, and the diffusion distance can reach 82.8 μm.
[0079] The microhardness of the nickel-based coating is 212.8 HV 0.2 , the conductivity is 17.52% IACS, and the volume formed under the current ablation of 180A is 2.01×10 7 μm 3 ablation pits.
[0080] Embodiment 3:
[0081] This embodiment provides a method for preparing a nickel-based coating by high-speed laser cladding on a copper alloy surface, the method comprising the following steps:
[0082] (1) sandblasting the surface of the copper alloy, wherein the sandblasting is performed by spraying the surface of the copper alloy with sand particles, wherein the sand particles are silicon nitride particles, and the average particle size of the sand particles is 100 meshes, the spraying angle of the sandblasting is 60 degrees, and the spraying pressure is 0.3 MPa. The sandblasting is stopped after the surface roughness of the copper alloy reaches 20 μm, and then ultrasonic cleaning is performed, wherein anhydrous ethanol is used as a cleaning medium during the ultrasonic cleaning, the power of the ultrasonic cleaning is 40 W, and the time is 10 min, to obtain a pretreated copper alloy substrate;
[0083] (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the raw material used for the high-speed laser cladding is nickel-based powder, which is a mixed powder of nickel powder and aluminum powder, wherein the mass fraction of nickel in the nickel-based powder is 88wt%, and the average particle size is 100μm, and the nickel-based powder is sprayed by coaxial powder feeding. The laser power during the high-speed laser cladding is 3250W, the laser scanning speed is 8m / min, the working distance is 22mm, the laser spot diameter is 2.5mm, the scanning path is an S-shaped reciprocating movement, and the overlap rate is 60%; the powder feeding flow rate during the high-speed laser cladding is 7.5g / min, the nickel-based powder is mixed with powder feeding gas nitrogen and then sprayed, and the flow rate of the powder feeding gas is 12L / min. During the high-speed laser cladding, a protective gas is introduced, and the protective gas is nitrogen, and its flow rate is 14L / min. After the high-speed laser cladding is completed, it is placed in the air for natural cooling to obtain a nickel-based coating, and the thickness of the nickel-based coating is 600μm.
[0084] The test method of the nickel-based coating refers to the test method in Example 1.
[0085] In this embodiment, the nickel-based coating prepared by the above method has a smooth surface, a dense internal structure, and no obvious defects. The interface between the copper alloy substrate and the nickel-based coating is obviously metallurgically bonded, and the diffusion distance can reach 66.3 μm.
[0086] The microhardness of the nickel-based coating is 181.3 HV 0.2 , the conductivity is 18.60% IACS, and the volume formed under the current ablation of 180A is 2.33×10 7 μm 3 ablation pits.
[0087] Embodiment 4:
[0088] This embodiment provides a method for preparing a nickel-based coating by high-speed laser cladding on a copper alloy surface, the method comprising the following steps:
[0089] (1) sandblasting the surface of the copper alloy, wherein the sandblasting is performed by spraying the surface of the copper alloy with sand particles, wherein the sand particles are silicon carbide particles, and the average particle size of the sand particles is 200 meshes, the spraying angle of the sandblasting is 40 degrees, and the spraying pressure is 0.45 MPa. The sandblasting is stopped after the surface roughness of the copper alloy reaches 10 μm, and then ultrasonic cleaning is performed, wherein acetone is used as the cleaning medium during the ultrasonic cleaning, the power of the ultrasonic cleaning is 45 W, and the time is 6 minutes, to obtain a pretreated copper alloy substrate;
[0090] (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the raw material used for the high-speed laser cladding is nickel-based powder, the nickel-based powder is a core-shell structure powder of aluminum-coated nickel, the mass fraction of nickel in the nickel-based powder is 95wt%, and the average particle size is 63μm. The nickel-based powder is sprayed by coaxial powder feeding. The laser power during the high-speed laser cladding is 3500W, the laser scanning speed is 9m / min, the working distance is 20.5mm, the laser spot diameter is 2.4mm, the scanning path is an S-shaped reciprocating movement, and the overlap rate is 65%; the powder feeding flow rate during the high-speed laser cladding is 4.6g / min, the nickel-based powder is mixed with argon powder feeding gas and then sprayed, the flow rate of the powder feeding gas is 8L / min, and a protective gas is introduced during the high-speed laser cladding, the protective gas is argon, and its flow rate is 11L / min. After the high-speed laser cladding is completed, it is placed in the air for natural cooling to obtain a nickel-based coating, and the thickness of the nickel-based coating is 450μm.
[0091] The test method of the nickel-based coating refers to the test method in Example 1.
[0092] In this embodiment, the nickel-based coating prepared by the above method has a smooth surface, a dense internal structure, and no obvious defects. The interface between the copper alloy substrate and the nickel-based coating is obviously metallurgically bonded, and the diffusion distance can reach 89.2 μm.
[0093] The microhardness of the nickel-based coating is 213.8 HV 0.2 , the conductivity is 17.30% IACS, and the volume formed under the current ablation of 180A is 2.08×10 7 μm 3 ablation pits.
[0094] Embodiment 5:
[0095] This embodiment provides a method for preparing a nickel-based coating by high-speed laser cladding on a copper alloy surface, the method comprising the following steps:
[0096] (1) sandblasting the surface of the copper alloy, wherein the sandblasting is performed by spraying the surface of the copper alloy with sand particles, wherein the sand particles are glass sand particles, and the average particle size of the sand particles is 180 meshes, the spraying angle of the sandblasting is 50 degrees, and the spraying pressure is 0.35 MPa. The sandblasting is stopped after the surface roughness of the copper alloy reaches 16 μm, and then ultrasonic cleaning is performed, wherein acetone is used as the cleaning medium during the ultrasonic cleaning, the power of the ultrasonic cleaning is 50 W, and the time is 7 minutes, to obtain a pretreated copper alloy substrate;
[0097] (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the raw material used for the high-speed laser cladding is nickel-based powder, which is a mixed powder of nickel powder and aluminum powder, wherein the mass fraction of nickel in the nickel-based powder is 85wt%, and the average particle size is 88μm, and the nickel-based powder is sprayed by coaxial powder feeding. The laser power during the high-speed laser cladding is 2500W, the laser scanning speed is 4.8m / min, the working distance is 21.5mm, the laser spot diameter is 2.1mm, the scanning path is an S-shaped reciprocating movement, and the overlap rate is 75%; the powder feeding flow rate during the high-speed laser cladding is 6g / min, the nickel-based powder is mixed with argon powder feeding gas and then sprayed, and the flow rate of the powder feeding gas is 9L / min, and a protective gas is introduced during the high-speed laser cladding, and the protective gas is argon gas, and its flow rate is 13L / min. After the high-speed laser cladding is completed, it is placed in the air for natural cooling to obtain a nickel-based coating, and the thickness of the nickel-based coating is 550μm.
[0098] The test method of the nickel-based coating refers to the test method in Example 1.
[0099] In this embodiment, the nickel-based coating prepared by the above method has a smooth surface, a dense internal structure, and no obvious defects. The interface between the copper alloy substrate and the nickel-based coating is obviously metallurgically bonded, and the diffusion distance can reach 86.2 μm.
[0100] The microhardness of the nickel-based coating is 196.8 HV 0.2 , the conductivity is 17.08% IACS, and the volume formed under the current ablation of 180A is 2.21×10 7 μm 3 ablation pits.
[0101] Comparative Example 1:
[0102] This comparative example provides a method for preparing a nickel-based coating on a copper alloy surface by high-speed laser cladding. The method refers to the method in Example 1, with the only difference being that the laser power in step (2) is 2000 W.
[0103] Comparative Example 2:
[0104] This comparative example provides a method for preparing a nickel-based coating on a copper alloy surface by high-speed laser cladding. The method refers to the method in Example 1, with the only difference being that the laser scanning speed in step (2) is 10 m / min.
[0105] In the above two comparative examples, due to the low laser power or the fast laser scanning speed during high-speed laser cladding, the heat input of the laser will be too small, which will cause insufficient melting of the powder, and the micro-molten pool formed on the surface of the copper substrate will be small in size, resulting in discontinuous coating formation and uneven surface. The surface roughness of the nickel-based coating reaches about 38.5μm, and defects such as pores are easily generated when the coating is combined with the interface.
[0106] Comparative Example 3:
[0107] This comparative example provides a method for preparing a nickel-based coating on a copper alloy surface by high-speed laser cladding. The method refers to the method in Example 1, with the only difference being that the laser power in step (2) is 4000 W.
[0108] Comparative Example 4:
[0109] This comparative example provides a method for preparing a nickel-based coating on a copper alloy surface by high-speed laser cladding. The method refers to the method in Example 1, with the only difference being that the laser scanning speed in step (2) is 4 m / min.
[0110] In the above two comparative examples, due to the high laser power or slow laser scanning speed during high-speed laser cladding, the heat input of the laser is too large, which leads to excessive melting of the powder. The micro-melting pool formed on the surface of the copper substrate is large, which makes the internal oxidation of the coating serious, the dilution rate is high, and the performance of the nickel-based coating is reduced. At this time, the microhardness of the nickel-based coating is 153.4HV. 0.2 , the conductivity is 7.23% IACS, and the volume formed under the current ablation of 180A is 4.28×10 7 μm 3 ablation pits.
[0111] It can be seen from the above embodiments and comparative examples that the high-speed laser cladding method of the present invention adopts a coaxial powder feeding method to prepare a nickel-based coating, and there is no need to adopt a prefabricated powder method, which can greatly simplify the process, shorten the preparation time, and improve the preparation efficiency. In addition, only a micro-molten pool is formed on the surface of the substrate, and the required laser energy is small, and the thermal impact on the copper alloy is also small; the method can effectively control the heat input of the laser by controlling the high-speed laser cladding process parameters to promote the full melting of the powder, ensure the high internal quality and defect-free coating, and promote the diffusion of interface elements in the coating forming process through the formation of a surface micro-molten pool, ensure the dense bonding and high bonding strength between the coating and the substrate, and the coating has excellent performance; the cooling rate after the laser cladding is relatively high, which can promote the refinement of the internal structure of the coating and further improve the coating performance; the method has a simple process flow, is easy to operate, has a low cost, and has a wider range of applications.
[0112] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the method of the present invention, addition of auxiliary steps, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a nickel-based coating on a copper alloy surface by high-speed laser cladding, characterized in that: The method comprises the following steps: (1) sandblasting the surface of the copper alloy, and then cleaning it to obtain a pretreated copper alloy substrate; (2) High-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the high-speed laser cladding adopts a coaxial powder feeding method, a laser power of 2500 to 3500 W, and a laser scanning speed of 4.8 to 9 m / min to prepare a nickel-based coating.
2. The method according to claim 1, characterized in that The copper alloy in step (1) includes any one of oxide dispersion strengthened copper, zirconium copper alloy or nickel copper alloy, or a combination of at least two thereof; Preferably, the copper alloy in step (1) is used as a component of a continuous casting crystallizer, a blast furnace tuyere or an electrical contact.
3. The method according to claim 1 or 2, characterized in that: The sandblasting treatment in step (1) is to spray the copper alloy surface with sand particles; Preferably, the sand particles include any one of aluminum oxide particles, glass sand, silicon carbide particles or silicon nitride particles, or a combination of at least two thereof; Preferably, the particle size of the sand particles is 80 to 200 meshes; Preferably, the spray angle of the sandblasting in step (1) is 30 to 60 degrees; Preferably, the spray pressure of the sandblasting treatment in step (1) is 0.3-0.5 MPa; Preferably, the sandblasting in step (1) is stopped after the roughness of the copper alloy surface reaches 10 to 20 μm.
4. The method according to any one of claims 1 to 3, characterized in that: The cleaning method in step (1) includes ultrasonic cleaning; Preferably, an organic solvent is used as a cleaning medium during the ultrasonic cleaning; Preferably, the organic solvent comprises ethanol and / or acetone; Preferably, the power of the ultrasonic cleaning is 25 to 50 W; Preferably, the ultrasonic cleaning time is 5 to 10 minutes.
5. The method according to any one of claims 1 to 4, characterized in that: The raw material used in the high-speed laser cladding in step (2) includes nickel-based powder; Preferably, the nickel-based powder is a core-shell structure powder of aluminum-coated nickel or a mixed powder of nickel powder and aluminum powder; Preferably, the mass fraction of nickel in the nickel-based powder is 85 to 95 wt %; Preferably, the particle size of the nickel-based powder is 53-106 μm.
6. The method according to any one of claims 1 to 5, characterized in that: The high-speed laser cladding in step (2) is performed using high-speed laser cladding equipment; Preferably, the laser cladding head of the high-speed laser cladding equipment uses an annular powder feeding nozzle for powder delivery; Preferably, during the high-speed laser cladding, the distance between the end of the laser cladding head and the surface of the copper alloy substrate is 20-22 mm.
7. The method according to any one of claims 1 to 6, characterized in that: The laser spot diameter during the high-speed laser cladding in step (2) is 2 to 2.5 mm; Preferably, the scanning path of the laser is a reciprocating movement along an S-shape; Preferably, the overlap rate between single tracks during laser scanning is 60-80%.
8. The method according to any one of claims 1 to 7, characterized in that: The powder feeding rate during the high-speed laser cladding in step (2) is 4.6 to 7.8 g / min; Preferably, the nickel-based powder is mixed with a powder feeding gas and then sprayed out, and the flow rate of the powder feeding gas is 7 to 12 L / min; Preferably, a protective gas is introduced during the high-speed laser cladding, and the flow rate of the protective gas is 10 to 15 L / min; Preferably, the powder feeding gas is ejected from a powder feeding port of a nozzle of the laser cladding head, and the shielding gas is ejected from the middle of the nozzle of the laser cladding head; Preferably, the powder feeding gas and the protective gas independently include inert gas and / or nitrogen.
9. The method according to any one of claims 1 to 8, characterized in that: After the high-speed laser cladding in step (2) is completed, the cladding is placed in air for natural cooling; Preferably, the thickness of the nickel-based coating in step (2) is 400-600 μm.
10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) sandblasting the copper alloy surface, wherein the sandblasting is performed by spraying the copper alloy surface with sand particles, wherein the sand particles include any one of aluminum oxide particles, glass sand, silicon carbide particles, or silicon nitride particles, or a combination of at least two of the particles, wherein the particle size of the sand particles is 80 to 200 meshes, the spraying angle of the sandblasting is 30 to 60 degrees, and the spraying pressure is 0.3 to 0.5 MPa. The sandblasting is stopped after the roughness of the copper alloy surface reaches 10 to 20 μm, and then ultrasonic cleaning is performed, wherein an organic solvent is used as a cleaning medium, the power of the ultrasonic cleaning is 25 to 50 W, and the time is 5 to 10 min, to obtain a pretreated copper alloy substrate; (2) high-speed laser cladding is performed on the surface of the copper alloy substrate pretreated in step (1), wherein the raw materials used for the high-speed laser cladding include nickel-based powder, wherein the nickel-based powder is a core-shell structure powder of aluminum-coated nickel or a mixed powder of nickel powder and aluminum powder, wherein the mass fraction of nickel in the nickel-based powder is 85-95wt%, and the particle size is 53-106μm, and the nickel-based powder is sprayed by coaxial powder feeding. The laser power during the high-speed laser cladding is 2500-3500W, the laser scanning speed is 4.8-9m / min, and the working distance is 20-22mm. The laser spot diameter is 2-2.5 mm, the scanning path is to move back and forth along an S-shape, and the overlap rate is 60-80%; the powder feeding flow rate during the high-speed laser cladding is 4.6-7.8 g / min, the nickel-based powder is mixed with the powder feeding gas and then sprayed out, the flow rate of the powder feeding gas is 7-12 L / min, and the protective gas is introduced during the high-speed laser cladding, and the flow rate of the protective gas is 10-15 L / min. After the high-speed laser cladding is completed, it is placed in the air for natural cooling to obtain a nickel-based coating, and the thickness of the nickel-based coating is 400-600 μm.
Citation Information
Patent Citations
Method for laser cladding of self-fluxing nickel-based alloy powder on copper alloy glass mold
CN116083914A
Method for reducing reflectivity during laser cladding of copper alloy matrix
CN116555757A
Cited By
Efficient laser cladding preparation method for nickel-based superalloy on surface of copper alloy
CN121131784A