Method for preparing catalytic electrode through environment-friendly degradation of PET waste plastics and application of catalytic electrode
A green hydrolysis method synthesizes MOF electrodes from PET waste, addressing low recycling rates and toxic solvent issues, achieving efficient ethylene glycol conversion and high-value product production.
Patent Information
- Application Number
- CN202411149511.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-03
AI Technical Summary
Current recycling methods for PET plastics face challenges such as low recycling rates, environmental pollution, and inefficient conversion of terephthalic acid (TPA) into high-value products, with existing electrocatalytic methods focusing mainly on ethylene glycol (EG) rather than TPA, and requiring toxic solvents for MOF synthesis.
A green alkaline hydrolysis method is used to directly synthesize metal-organic framework (MOF) catalytic electrodes from waste PET plastics, employing a three-electrode system with HgO/Hg and platinum sheet electrodes, and a hydrothermal reaction to convert PET into MOF materials, which are then used for ethylene glycol electro-oxidation.
This method efficiently converts PET waste into high-value MOF materials, reducing environmental impact and enhancing ethylene glycol electro-oxidation performance, producing high-value products with reduced overpotential.
Smart Images

Figure CN119061422A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycling waste PET plastics, and specifically relates to a method for preparing a catalytic electrode by green degradation of waste PET plastics and an application thereof. Background Art
[0002] Polyethylene terephthalate (PET) is a polymer synthesized by the dehydration condensation reaction of terephthalic acid (TPA) and ethylene glycol (EG), with an annual output of up to 70 million tons. Due to its excellent physical and chemical properties, PET is widely used in the fields of packaging materials and textiles. However, the recycling rate of PET plastic products is only about 20%, and most of them are landfilled or discarded, which not only causes environmental pollution, but also causes a large amount of waste of carbon resources. The commonly used methods at present are physical recycling, which has high requirements for the purity of waste PET and has problems such as degradation of the quality of recycled products. The chemical recycling method refers to the PET depolymerization reaction, which can completely depolymerize PET into monomers terephthalic acid (TPA) and ethylene glycol (EG) under specific conditions, but common methods such as hydrolysis, alcoholysis and glycolysis have problems such as equipment corrosion, high cost and low product purity.
[0003] In recent years, electrocatalytic upgrading as a recycling method for waste PET has attracted widespread attention due to renewable electricity and mild operating conditions. The basic principle is to depolymerize PET under alkaline conditions to obtain terephthalate and ethylene glycol, and then use alkaline ethylene glycol solution as an electrolyte to carry out electrochemical reforming under the action of a catalyst to oxidize EG into high-value chemicals such as formate, glycolate and oxalate. For example, Duan Haohong's team at Tsinghua University constructed a transition metal phosphide (CoNi 0.25 P / NF) as a bifunctional catalyst to achieve the upgrading and recycling of waste PET plastics to generate high value-added TPA, potassium diformate (KDF) and H2 fuel. However, current research mainly focuses on the upgrading and utilization of EG, a monomer derived from the depolymerization of waste PET plastics, but there is relatively little research on the upgrading and utilization of another important depolymerization monomer TPA. In fact, TPA is a common organic ligand in the synthesis of metal-organic framework materials (MOFs) such as MIL-101, UIO-66 and MOF-5. MOF is a class of crystalline porous materials with high specific surface area, high porosity and structural designability, and shows great development potential as a new type of electrocatalyst.
[0004] Using PET plastic as a ligand source to construct MOF usually involves tedious depolymerization, purification and solvent methods. In addition, the solvothermal method requires the use of toxic organic solvents (such as DMF, triethylamine, etc.). Therefore, it is of great practical significance to develop a green method with simple process and no organic solvent to convert waste PET plastic into functional MOF materials. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a method for synthesizing high-performance metal-organic framework catalytic electrodes by degrading waste PET waste plastics through a green alkaline hydrolysis method, thereby reducing environmental pollution and completing the upgrading and recycling of PET waste plastics, while achieving electrocatalysis of ethylene glycol and upgrading it to high value-added products.
[0006] The purpose of the present invention can be achieved by the following technical scheme: PET waste plastic is degraded by green solvent thermal to prepare metal-organic framework / NF directly as a working electrode, HgO / Hg is used as a reference electrode, and a platinum sheet electrode is used as a counter electrode to form a three-electrode system to catalyze the electro-oxidation reaction of ethylene glycol in an H-type electrolytic cell. The specific steps of the green decomposition of waste PET and the high-value recovery of ethylene glycol are as follows:
[0007] (1) dissolving a metal salt in deionized water to form an initial solution;
[0008] The metal salt is selected from at least one of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, ferrous sulfate heptahydrate, ferric chloride hexahydrate, cobalt chloride, copper nitrate and zinc nitrate; the added amount of the metal salt is 0.5-2 mmol.
[0009] (2) The alkaline substance is mixed with the initial solution to form an ideal medium;
[0010] The alkaline substance may include sodium hydroxide, sodium carbonate, sodium bicarbonate, ammonia water, etc. The amount of the alkaline substance added is 0.1 to 3 mmol.
[0011] (3) The pretreated nickel foam is used as a supporting substrate, and PET waste plastic is placed in a solution for a hydrothermal reaction; a MOF catalytic material rich in metal ions is in situ grown on the surface of the nickel foam;
[0012] The PET waste plastic is a film sheet or a polyester material; the amount of the PET waste plastic added is 0.1 to 0.5 g.
[0013] Before using nickel foam NF, it should be ultrasonically cleaned in acetone, hydrochloric acid, and ethanol to remove surface oil and oxides, otherwise the material will not grow evenly on the surface of NF;
[0014] The temperature of the hydrothermal reaction is 160-180°C, and the reaction time is 12-36 hours.
[0015] (4) After the reaction is completed, the MOF catalytic material rich in metal ions is washed and dried to finally obtain a catalytic electrode.
[0016] The metal-organic framework catalytic electrode prepared by the above method is used as a working electrode to catalyze the electro-oxidation reaction of ethylene glycol.
[0017] When the electrolytic reaction system is electrolyzed, the applied electrolytic cell voltage ranges from 0.8 to 2V.
[0018] The electrolyte is a mixed solution of alkaline solution and ethylene glycol, and the alkaline solution includes KOH; preferably, the concentration of the alkaline solution is 1-1.5M, and preferably, the concentration of the ethylene glycol solution is 0.1-0.5M.
[0019] Beneficial effects: By adopting a green and simple one-step hydrothermal synthesis method, an efficient ethylene glycol electro-oxidation working electrode was synthesized directly from waste PET plastics and cheap metal salts on a nickel foam substrate. This method not only solves the problems existing in the traditional recycling of PET plastics, but also realizes the concept of "turning waste into treasure" - that is, by reacting the decomposed terephthalic acid with metal salts to generate MOF (metal organic framework) materials; and this MOF material can significantly reduce the overpotential of ethylene glycol electro-oxidation, while producing products with high added value, which is of great significance for promoting sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 XRD spectra of Co-MOF / NF(NaOH), Co-MOF / NF(BDC), Co-MOF / NF(PET), and Co(OH)2 / NF prepared in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3;
[0021] Figure 2 The scanning electron microscope images of Co-MOF / NF(NaOH), Co-MOF / NF(BDC), and Co-MOF / NF(PET) prepared in Example 1, Comparative Example 1, and Comparative Example 2 are shown in FIG. (a).
[0022] Co-MOF / NF (PET), (b) Co-MOF / NF (BDC), (c) Co-MOF / NF (NaOH).
[0023] Figure 3 The LSV, EIS, and C of the electrolytic water oxygen evolution reaction of Co-MOF / NF(NaOH), Co-MOF / NF(BDC), Co-MOF / NF(PET), and Co(OH)2 / NF prepared in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 are shown in FIG. dl and overpotential comparison diagram; where (a) LSV, (b) overpotential at different current densities, (c) C dl , (d) EIS. DETAILED DESCRIPTION
[0024] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0025] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0026] Example 1
[0027] NF pretreatment:
[0028] Before using NF, it should be ultrasonically cleaned in acetone, hydrochloric acid, and ethanol for 15 minutes each. Otherwise, the oil and oxide on the surface of industrial NF will prevent the material from growing evenly on the NF surface.
[0029] All reaction solutions are prepared and used immediately, and the reaction solutions need to be fully mixed by ultrasound or stirring.
[0030] This step is applicable to all the following embodiments and comparative examples.
[0031] Preparation of Co-MOF / NF(NaOH) electrode:
[0032] Add 20mL of deionized water and 291mg of solid cobalt nitrate hexahydrate to a 50mL beaker to form solution A; add 80mg of solid sodium hydroxide to solution A and mix well to form solution B. Transfer the above solution B to a 50mL high-temperature reactor, immerse 1cm×3cm of NF and 0.2g of PET waste plastic in the above solution, seal it, and react it in a constant temperature oven at 170℃ for 24h. After the reaction, rinse the electrode with deionized water and ethanol several times until there is no obvious impurity on the surface, then put it in a constant temperature oven, dry it at 60℃ for 24h, and cool it to room temperature to obtain a Co-MOF / NF (NaOH) electrode with a nanosheet structure.
[0033] Figure 1 This is the XRD diagram of the Co-MOF / NF (NaOH) electrode. It can be seen from the figure that the XRD diffraction peak of the prepared Co-MOF / NF (NaOH) electrode corresponds to Co-MOF.
[0034] Figure 2c shows the SEM image of the prepared Co-MOF / NF (NaOH) electrode, and the structure of the prepared material was characterized and analyzed. From the figure, it can be observed that the electrode surface obtained by the hydrothermal reaction is covered with a dense nanosheet structure, indicating that a Co-MOF / NF (NaOH) electrode with a three-dimensional nanosheet array structure was successfully prepared.
[0035] Example 2
[0036] Preparation of Fe-MOF / NF(NaOH) electrode:
[0037] Add 20 mL of deionized water and 278 mg of solid ferrous sulfate heptahydrate to a 50 mL beaker to form solution A; add 80 mg of solid sodium hydroxide to solution A and mix well to form solution B. Transfer the above solution B to a 50 mL high temperature reactor, immerse 1 cm × 3 cm NF and 0.2 g of PET waste plastic in the above solution, seal it, and react in a constant temperature oven at 170 ° C for 24 hours. After the reaction is completed, rinse the electrode with deionized water and ethanol for multiple times, then put it in a constant temperature oven, dry it at 60 ° C for 24 hours, and cool it to room temperature to obtain the Fe-MOF / NF (NaOH) electrode.
[0038] Example 3
[0039] Preparation of Ni-MOF / NF(NaOH) electrode:
[0040] Add 20 mL of deionized water and 291 mg of nickel nitrate hexahydrate solid to a 50 mL beaker to form solution A; add 80 mg of sodium hydroxide solid to solution A and mix well to form solution B. Transfer the above solution B to a 50 mL high temperature reactor, immerse 1 cm × 3 cm of NF and 0.2 g of PET waste plastic in the above solution, seal it, and react in a constant temperature oven at 170 ° C for 24 hours. After the reaction is completed, rinse the electrode with deionized water and ethanol several times, then put it in a constant temperature oven, dry it at 60 ° C for 24 hours, and cool it to room temperature to obtain a Ni-MOF / NF (NaOH) electrode.
[0041] Example 4
[0042] Preparation of Co-MOF / NF(NaOH)-180℃ electrode
[0043] Add 20mL of deionized water and 291mg of cobalt nitrate hexahydrate to a 50mL beaker to form solution A; add 80mg of sodium hydroxide solid to solution A and mix well to form solution B. Transfer the above solution B to a 50mL high-temperature reactor, immerse 1cm×3cm of NF and 0.2g of PET waste plastic in the above solution, seal it, and react at 180℃ in a constant temperature oven for 24h. After the reaction, rinse the electrode with deionized water and ethanol several times, then put it in a constant temperature oven, dry it at 60℃ for 24h, and cool it to room temperature to obtain a Co-MOF / NF(NaOH)-180℃ electrode with a nanosheet structure.
[0044] Example 5
[0045] Preparation of Co-MOF / NF(NaOH)-1 electrode
[0046] Add 20mL of deionized water and 291mg of cobalt nitrate hexahydrate to a 50mL beaker to form solution A; add 40mg of sodium hydroxide solid to solution A and mix well to form solution B. Transfer the above solution B to a 50mL high-temperature reactor, immerse 1cm×3cm of NF and 0.2g of PET waste plastic in the above solution, seal it, and react in a constant temperature oven at 170℃ for 24h. After the reaction, rinse the electrode with deionized water and ethanol several times, then put it in a constant temperature oven, dry it at 60℃ for 24h, and cool it to room temperature to obtain a Co-MOF / NF(NaOH)-1 electrode with a nanosheet structure.
[0047] Example 6
[0048] Preparation of Co-MOF / NF(NaOH)-3 electrode
[0049] Add 20mL of deionized water and 291mg of cobalt nitrate hexahydrate to a 50mL beaker to form solution A; add 120mg of sodium hydroxide solid to solution A and mix well to form solution B. Transfer the above solution B to a 50mL high-temperature reactor, immerse 1cm×3cm of NF and 0.2g of PET waste plastic in the above solution, seal it, and react in a constant temperature oven at 170℃ for 24h. After the reaction, rinse the electrode with deionized water and ethanol several times, then put it in a constant temperature oven, dry it at 60℃ for 24h, and cool it to room temperature to obtain a Co-MOF / NF(NaOH)-3 electrode with a nanosheet structure.
[0050] Example 7
[0051] Preparation of Co-MOF / NF(Na2CO3) electrode
[0052] 80 mg of sodium hydroxide solid and 291 mg of cobalt nitrate hexahydrate were replaced with 80 mg of anhydrous sodium carbonate and 291 mg of cobalt nitrate hexahydrate. The other preparation processes were the same as in Example 1 to obtain a Co-MOF / NF (Na2CO3) electrode.
[0053] This indicates that Co-MOF / NF(Na2CO3) was successfully prepared. Its 100mA cm -2 The EGOR performance under the above conditions is shown in Table 1.
[0054] Example 8
[0055] Preparation of Co-MOF / NF(NaHCO3) electrode
[0056] 80 mg of sodium hydroxide solid and 291 mg of cobalt nitrate hexahydrate were replaced with 80 mg of anhydrous sodium bicarbonate and 291 mg of cobalt nitrate hexahydrate. The other preparation processes were the same as in Example 1 to obtain a Co-MOF / NF (NaHCO3) electrode.
[0057] This indicates that Co-MOF / NF(NaHCO3) was successfully prepared. Its 100mA cm -2 The EGOR performance under the above conditions is shown in Table 1.
[0058] Comparative Example 1
[0059] The 0.3 g PET in Example 5 was replaced by 166 mg terephthalic acid, and the other preparation processes were the same as in Example 5 to obtain a Co-MOF / NF (BDC) electrode.
[0060] Comparative Example 2
[0061] Preparation of Co-MOF / NF(PET) electrode
[0062] Add 10mL of deionized water and 291mg of cobalt nitrate hexahydrate to a 50mL beaker to form solution A; add 3mL of H2O and 4mL of DMF to solution A and mix well to form solution B. Transfer the above solution B to a 50mL high-temperature reactor, immerse 1cm×3cm of NF and 0.3g of PET waste plastic in the above solution, seal it, and react in a constant temperature oven at 170℃ for 24h. After the reaction, rinse the electrode with deionized water and ethanol several times, then put it in a constant temperature oven, dry it at 60℃ for 24h, and cool it to room temperature to obtain a Co-MOF / NF (PET) electrode with a nanosheet structure. Figure 2a shows the SEM image of the prepared Co-MOF / NF(PET) electrode, and the structure of the prepared material was characterized and analyzed. From the figure, it can be seen that the electrode surface obtained by hydrothermal reaction is covered with a uniform nanosheet structure, indicating that Co-MOF / NF(PET) with a cutting-edge nanosheet structure has been successfully prepared. -2 The EGOR performance under the above conditions is shown in Table 1.
[0063] Comparative Example 3
[0064] Preparation of Co(OH)2 / NF electrode
[0065] Add 30 mL of H2O to 436 mg of cobalt nitrate hexahydrate and 120 mg of urea, mix well, and form a mixed solution. Transfer the above solution into a 50 mL high temperature reactor, immerse 1 cm × 3 cm of NF in the above solution, seal, and react in a constant temperature oven at 120 ° C for 10 hours. After the reaction, rinse the electrode with deionized water and ethanol several times, then put it in a constant temperature oven, dry it at 60 ° C for 24 hours, and cool it to room temperature to obtain a Co(OH)2 / NF electrode with a nanowire structure.
[0066] Figure 2 b shows the SEM image of the prepared Co-MOF / NF(BDC) electrode. The structure of the prepared material was characterized and analyzed. From the figure, it can be seen that the electrode surface obtained by hydrothermal reaction is covered with a uniform nanoblock structure, indicating that Co-MOF / NF(BDC) with a cutting-edge nanoblock structure was successfully prepared. Its 100 mA cm -2 The EGOR performance under the above conditions is shown in Table 1.
[0067] Table 1 Comparison of EGOR performance under different conditions and metal salts
[0068]
[0069] Application Examples
[0070] The three-electrode system was composed of the electrodes prepared in Examples 1 to 8 as working electrodes, the HgO / Hg electrode as reference electrode, and the platinum sheet electrode as counter electrode, and the electrocatalytic activity test was carried out. The specific steps are as follows:
[0071] The electrochemical performance was tested using a three-electrode system, with the electrode prepared in the present invention as the working electrode, the HgO / Hg electrode as the reference electrode, and the platinum sheet electrode as the counter electrode. The effective area of the working electrode was 0.2 cm 2 The electrolyte was a mixture of 1 M KOH solution and 0.5 M ethylene glycol. The scan rate of the CV test was 5 mV s -1, the EIS test voltage is 0.3V, and the experimental test temperature is room temperature.
[0072] Test results such as Figure 3 As shown in Figure 2, Co-MOF / NF(NaOH) has the best EGOR catalytic performance, for example, achieving 100 mA cm -2 The current density overpotential is only 1.32V vs. RHE, which saves 200mV compared with blank NF. In addition, the interfacial transport kinetics was studied by electrochemical impedance spectroscopy (EIS). Figure 3 d shows that in the electrochemical impedance spectroscopy, the charge transfer resistance (R ct ) can reflect the energy loss caused by electron transfer between electrochemical reactants and is an important parameter for evaluating electrochemical catalysts. Although the semicircle of Co-MOF / NF(NaOH) in the EIS graph is similar to that of Co-MOF / NF(PET) and Co-MOF / NF(BDC), the MOF synthesized using this green depolymerization method can have similar charge transfer impedance, proving that it has an equivalent electron transfer speed. And combined with Figure 3 c Joint analysis, double layer capacitance (C dl ) shows that the electrochemical active area of Co-MOF / NF(NaOH) is larger than that of the other three materials. The results show that Co-MOF / NF(NaOH) is a greener and more efficient catalytic material for EGOR reaction.
[0073] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing catalytic electrodes by green degradation of PET waste plastics, characterized in that: The method steps are as follows: (1) dissolving a metal salt in pure deionized water to prepare an initial solution, and then adding an alkaline reagent to the initial solution to prepare a reaction medium; (2) using the pretreated nickel foam as a supporting substrate and immersing it together with the waste PET plastic sheet into the reaction medium of step (1) to perform a hydrothermal reaction, thereby in situ growing a MOF catalytic material rich in metal ions on the surface of the nickel foam; (3) After the reaction is completed, the MOF catalytic material rich in metal ions is washed and dried to finally obtain a catalytic electrode.
2. The method for preparing catalytic electrodes by green degradation of PET waste plastics as claimed in claim 1, characterized in that: The metal salt is at least one of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, ferrous sulfate heptahydrate, ferric chloride hexahydrate, cobalt chloride, copper nitrate, and zinc nitrate; the alkaline reagent is at least one of sodium hydroxide, sodium carbonate, sodium bicarbonate, and ammonia water NH3·H2O.
3. The method for preparing catalytic electrodes by green degradation of PET waste plastics as claimed in claim 1, characterized in that: The PET waste plastic is one of a film sheet or a polyester material.
4. The method for preparing catalytic electrodes by green degradation of PET waste plastics as claimed in claim 1, characterized in that: The usage amount of the PET waste plastic is 0.1-0.5 g; the addition amount of the metal salt is 0.1-2 mmol; and the addition amount of the alkaline substance is 0.1-3 mmol.
5. The method for preparing catalytic electrodes by green degradation of PET waste plastics as claimed in claim 1, characterized in that: The temperature of the hydrothermal reaction is 160-180° C., and the reaction time is 12-36 hours.
6. A catalytic electrode prepared by the method according to any one of claims 1 to 5.
7. An application of a catalytic electrode prepared by the method according to any one of claims 1 to 5, characterized in that: The catalytic electrode is used for catalyzing the electro-oxidation reaction of ethylene glycol.
8. The use of the catalytic electrode according to claim 7, characterized in that: When the ethylene glycol electro-oxidation reaction is catalyzed, the applied electrolytic cell voltage ranges from 0.8 to 2V.
9. The use of the catalytic electrode according to claim 7, characterized in that: When the catalytic ethylene glycol electro-oxidation reaction is carried out, the electrolyte is an alkaline solution plus ethylene glycol, the concentration of the alkaline solution is 1-1.5M, and the concentration of the ethylene glycol solution is 0.1-0.5M.
Citation Information
Cited By
Method for green hydro-thermal synthesis of NiMn-MOF / NF electrode from waste plastics and application of NiMn-MOF / NF electrode
CN119707039A
Method for co-processing industrial sulfur-containing flue gas and upgrading and converting PET waste plastics into hydroxyl methane sulfonate through electro-catalysis
CN119736642A
Waste PET (polyethylene terephthalate)-based MOFs (metal organic frameworks) functional material as well as preparation method and application thereof