Preparation method of high-entropy ruthenium oxide oxygen evolution reaction catalyst

The highly entropy ruthenium oxide catalyst was prepared by hydrothermal method and vapor deposition method, which solved the solubility resistance of ruthenium oxide catalyst under high oxidation potential, and achieved high activity and high stability OER catalysts, which were suitable for energy catalytic conversion.

CN119061424AInactive Publication Date: 2024-12-03SHANDONG UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411556938.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing ruthenium oxide catalysts have poor solubility resistance at high oxidation potential, resulting in a short service life under harsh anode and acidic conditions, limiting their application in energy catalytic conversion.

Method used

Hydrothermal method and vapor deposition method are used to prepare highly entropy ruthenium oxide catalyst to form spherical nanoparticles with rough surfaces. By mixing a variety of metal salts and sodium hydroxide to dissolve, heat, centrifugation, drying and annealing, forming high entropy Ruthenium oxide catalyst.

Benefits of technology

It improves the OER activity and stability of the catalyst, increases the specific surface area and surface roughness, extends the service life of the catalyst, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061424A_ABST
    Figure CN119061424A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-entropy ruthenium oxide oxygen evolution reaction catalyst. The preparation method comprises the following steps: obtaining high-entropy ruthenium hydroxide by utilizing a hydrothermal method; and carrying out annealing treatment on the high-entropy ruthenium hydroxide to obtain the high-entropy ruthenium oxide. The microstructure of the catalyst is spherical nanoparticles, the catalyst has a high electrochemical active area and multiple electrochemical active sites, and the oxygen evolution reaction activity is greatly improved. In addition, due to the high-entropy effect generated by adding multiple elements, the catalyst has high catalytic stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrocatalytic energy materials, and in particular to a method for preparing a high-entropy ruthenium oxide oxygen evolution reaction catalyst. Background Art

[0002] The core reaction in energy catalytic conversion technologies such as water electrolyzer hydrogen production, metal-air batteries and fuel cells is the oxygen evolution reaction (OER). However, the oxygen evolution reaction (OER) has become a bottleneck in the development of energy catalytic conversion due to its complex four-electron transfer process that leads to sluggish kinetics. The activity and stability of the oxygen evolution reaction have become the key to sustainable energy development. In order to achieve both high activity and high stability of OER, it is necessary to explore efficient and durable OER electrocatalysts.

[0003] The most effective catalysts for accelerating OER kinetics are iridium oxide and ruthenium oxide. However, Ru will be over-oxidized to volatile RuO4 or soluble RuO5 at high oxidation potentials (>1.4 V). 2- , resulting in poor solubility of ruthenium oxide under harsh anode and acidic conditions, and its life span is only a few dozen hours, which is not conducive to large-scale commercial application. Therefore, it is very necessary to improve the working stability of ruthenium-based catalysts while maintaining their activity. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst, which has a simple preparation method and low cost, and has high activity and high stability for the oxygen evolution reaction.

[0005] The invention discloses a method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst, which comprises: preparing the high entropy ruthenium oxide oxygen evolution reaction catalyst by a hydrothermal method and a vapor deposition method, wherein the catalyst has a rough surface and is in the form of nanoparticles. The method comprises the following steps: (1) dissolving ruthenium chloride, vanadium chloride, chromium chloride, manganese chloride, nickel chloride and sodium hydroxide in deionized water to obtain a mixed solution; (2) heating the mixed solution by a hydrothermal method to obtain a high entropy ruthenium hydroxide solution; (3) centrifuging and drying the solution to obtain a high entropy ruthenium hydroxide powder; and (4) annealing the high entropy ruthenium hydroxide powder obtained in step (3) in an air atmosphere to obtain a high entropy ruthenium oxide catalyst.

[0006] The total content of ruthenium chloride, vanadium chloride, chromium chloride, manganese chloride and nickel chloride in step (1) is 0.4 mmol to 0.6 mmol.

[0007] In the step (1), the molar ratio of ruthenium chloride, vanadium chloride, chromium chloride, manganese chloride and nickel chloride is 1:0.5:0.5:0.5:0.5 to 1:2:2:2:2.

[0008] In the step (1), the amount of sodium hydroxide is 0.005 g to 0.015 g.

[0009] In the step (1), the amount of deionized water is 10 ml to 20 ml.

[0010] In the step (2), the mixed solution is heated at a temperature of 140° C. to 160° C. and for a heating time of 8 h to 12 h.

[0011] The speed of the centrifugal treatment in step (3) is 7500 r min -1 Up to 8500 rpm -1 The centrifugation time is 4 min to 6 min, the number of centrifugation times is 1 to 3 times, the drying temperature is 50 ℃ to 70 ℃, and the drying time is 3 h to 4 h.

[0012] The annealing temperature in step (4) is 550°C to 650°C, and the heating rate is 8°C min -1 to 12℃ min -1 , the annealing time is 0.5 h to 1.5 h.

[0013] In addition, the present invention also discloses a high entropy ruthenium oxide oxygen evolution reaction catalyst.

[0014] The high entropy ruthenium oxide oxygen evolution reaction catalyst prepared in the present invention is prepared by any of the above-mentioned methods for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst. The high entropy ruthenium oxide oxygen evolution reaction catalyst is a spherical nanoparticle with a particle size of 6.15 nm.

[0015] Compared with the prior art, the present invention has the following advantages.

[0016] (1) The high-entropy ruthenium oxide oxygen evolution reaction catalyst prepared by the preparation method of the present invention has excellent OER activity and stability; (2) Compared with catalysts with other morphologies, the catalyst prepared by the preparation method of the present invention is spherical nanoparticles with a larger specific surface area and surface roughness, which increases the number of OER active sites; (3) The preparation method of the present invention has a simple process and good repeatability, and can be prepared on a large scale to meet industrial needs; (4) The catalyst is mainly composed of ruthenium oxide, which ensures the OER activity of the catalyst; (5) The catalyst is a high-entropy material, which utilizes the entropy stabilization effect and hysteresis diffusion effect of the high-entropy material to effectively improve the OER stability of the ruthenium-based catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the X-ray diffraction pattern (XRD) of (VCrMnNiRu)O2 prepared in Example 1.

[0018] Figure 2 This is a scanning electron microscopy image (SEM) of (VCrMnNiRu)O2 prepared in Example 1.

[0019] Figure 3 This is the OER polarization curve of (VCrMnNiRu)O2 prepared in Example 1 in 0.5 M H2SO4 electrolyte.

[0020] Figure 4 is the Tafel slope of (VCrMnNiRu)O2 prepared in Example 1 in 0.5 M H2SO4 electrolyte.

[0021] Figure 5 This is the double layer capacitance curve of (VCrMnNiRu)O2 prepared in Example 1 in 0.5 M H2SO4 electrolyte.

[0022] Figure 6 This is the impedance diagram of (VCrMnNiRu)O2 prepared in Example 1 in 0.5 M H2SO4 electrolyte.

[0023] Figure 7 LSV curves of (VCrMnNiRu)O2 prepared in Example 1 after different number of cycles in 0.5 M H2SO4 electrolyte.

[0024] Figure 8 The voltage change diagram at different current densities obtained from the LSV curve of (VCrMnNiRu)O2 prepared in Example 1 after different number of cycles reflects the stability of (VCrMnNiRu)O2. DETAILED DESCRIPTION

[0025] The present invention uses RIGAKU SmartLab X-ray diffractometer to obtain XRD patterns. The instrument uses Cu Kα as the anode target, the X-ray power is 2 kW, and the scanning speed is 6 °min -1 , the scanning range is 10 °~80 °; the SEM images were obtained using a FEI Quanta-450 FEG field emission scanning electron microscope; the OER test was performed using a Chenhua electrochemical workstation, where the reference electrode was Ag / AgCl, the counter electrode was a carbon rod, the working electrode was a high entropy oxidized ruthenium catalyst, and the electrolyte was 0.5 M H2SO4. The IR compensation of the LSV polarization curve was 95%, the test voltage range was 0.8 V vs. Ag / AgCl to 1.5 V vs. Ag / AgCl, and the scanning speed was 2 mV s -1 The Tafel slope is obtained from the LSV polarization curve. The input voltage of the impedance is 0.45926 V vs. Ag / AgCl.

[0026] Embodiment 1:

[0027] (1) Dissolve 0.1 mmol ruthenium chloride, 0.1 mmol vanadium chloride, 0.1 mmol chromium chloride, 0.1 mmol manganese chloride, 0.1 mmol nickel chloride, and 0.25 mmol sodium hydroxide in 15 ml deionized water.

[0028] (2) The solution in step (1) was transferred into a 50 ml reaction kettle and kept at 150° C. for 10 h to obtain a high entropy ruthenium hydroxide solution.

[0029] (3) The solution in step (2) was transferred into a centrifuge at a speed of 8000 r / min. -1 The mixture was centrifuged at 400 °C for 5 min and centrifuged twice to obtain high entropy ruthenium hydroxide powder.

[0030] (4) The sample in step (3) was transferred into a vacuum drying oven and kept at 60° C. for 3.5 h to obtain a dry high-entropy ruthenium hydroxide powder.

[0031] (5) Annealing the catalyst obtained in step (4) in an air atmosphere (600° C., 1 h) to obtain a high-entropy ruthenium oxide catalyst.

[0032] FIG1 shows that the high entropy ruthenium oxide catalyst (VCrMnNiRu)O2 prepared by the present invention is consistent with the RuO2 standard card and has a single-phase structure without other impurities ( Figure 1 PDF#97-005-6007 in the table is a standard crystal card of RuO2).

[0033] FIG. 2 shows that the high entropy ruthenium oxide catalyst (VCrMnNiRu)O2 prepared by the present invention is spherical nanoparticles with a particle size of 6.15 nm.

[0034] The high entropy ruthenium oxide catalyst (VCrMnNiRu)O2 prepared by the present invention is used as a working electrode, a carbon rod is used as a counter electrode, Ag / AgCl is used as a reference electrode, and 0.5 M H2SO4 is used as an electrolyte. The electrochemical OER performance test of (VCrMnNiRu)O2 is performed, and the test results are shown in the figure. Figure 3 It shows that the (VCrMnNiRu)O2 catalyst of the present invention only needs a low overpotential of 216 mV to achieve 10 mA cm -2 The current density is much lower than that of commercial RuO2 (326 mV). Figure 4 The Tafel slope of the (VCrMnNiRu)O2 catalyst of the present invention is only 27.63 mV dec -1 , indicating that (VCrMnNiRu)O2 has very fast OER reaction kinetics. Figure 5 The double-layer capacitance curve of (VCrMnNiRu)O2 of the present invention is 28.7 mF cm -2 The high double-layer capacitance value shows that (VCrMnNiRu)O2 has a large electrochemically active surface area and many electrochemically active sites, which is beneficial to its OER activity. Figure 6 The electrochemical impedance spectrum of the (VCrMnNiRu)O2 catalyst of the present invention shows that the charge transfer resistance is only 16 Ω, indicating that it has a small charge transfer resistance value, which is beneficial to the electron transfer between the electrolyte and the catalyst surface and enhances the conductivity. Figure 7 It shows that after 500 CV cycles, the LSV polarization curves of the (VCrMnNiRu)O2 catalyst of the present invention are almost overlapped, there is no obvious activity decay, and it has excellent oxygen evolution stability. Figure 8 It is shown that in the LSV measurement, no sudden drop in potential is observed at any given current density, and the present invention has excellent oxygen evolution stability.

[0035] Compared with the prior art, the present invention improves the synthesis method of the catalyst. The method makes the catalyst preparation simple, improves the yield, has good repeatability, is suitable for large-scale production, and has significant green environmental protection benefits. The synthesis method enables the catalyst to have a higher catalyst specific surface area, provides abundant active sites that are conducive to electron transfer in the OER process, and improves the catalytic activity of the ruthenium oxide catalyst to a level higher than that of commercial ruthenium oxide. In addition, the synthesis method also improves the catalytic stability of the ruthenium oxide catalyst, which mainly depends on the high entropy effect generated by the addition of multiple elements. It can be widely used in the fields of water electrolysis, hydrogen production, and batteries.

[0036] Although the above embodiments of the present invention are described in conjunction with the accompanying drawings, it should be noted that the present invention is not limited to the above specific embodiments or application fields. In addition, the above description is only a preferred embodiment of the present invention, which is only for illustrative purposes and is not intended to limit the present invention. Individuals with a certain level of professional knowledge in this field can, under the inspiration of this description, make substitutions, improvements, etc. without departing from the scope of protection claimed by the present invention, which should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-entropy ruthenium oxide oxygen evolution reaction catalyst, comprising the following steps: adding vanadium chloride, chromium chloride, manganese chloride, nickel chloride, ruthenium chloride, and sodium hydroxide to deionized water, completely dissolving them to obtain a mixed solution, and heating the mixed solution by a hydrothermal method; centrifuging and drying the heated mixed solution to obtain a high-entropy ruthenium hydroxide catalyst; annealing the high-entropy ruthenium hydroxide catalyst to obtain a high-entropy ruthenium oxide catalyst; the total content of the vanadium chloride, chromium chloride, manganese chloride, nickel chloride, and ruthenium chloride is 0.4 mmol to 0.6 mmol.

2. The method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: The molar ratio of vanadium chloride, chromium chloride, manganese chloride, nickel chloride and ruthenium chloride is 1:0.5:0.5:0.5:0.5 to 1:2:2:2:

2.

3. The method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: The deionized water is 10 ml to 20 ml.

4. The method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: Sodium hydroxide is 0.005 g to 0.015 g.

5. The method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: The mixed solution is heated at a temperature of 140°C to 160°C, and the heating time is 8 h to 12 h.

6. The method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: The centrifugal speed was 7500 r min -1 Up to 8500 rpm -1 , the centrifugation time is 4 min to 6 min, and the number of centrifugation is 1 to 3 times.

7. The method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: The drying temperature is 50 ℃ to 70 ℃, and the drying time is 3 h to 4 h.

8. The method for preparing a high entropy ruthenium oxide oxygen evolution reaction catalyst according to claim 1, characterized in that: The annealing temperature is 550°C to 650°C, and the annealing time is 0.5 h to 1.5 h.

Citation Information

Patent Citations

  • Synthetic method of colored spinel type high-entropy oxide (NiFeCrM)3O4

    CN113511693A

  • Preparation method of (CoCuZnMnMg) 3O4 high-entropy oxide

    CN115518649A

  • Precious metal monatomic catalyst based on high-entropy effect and preparation method thereof

    CN115896810A

  • Preparation method of medium-high entropy alloy nanoflower catalyst

    CN116666633A

  • Manganese-doped ruthenium oxide nano-catalyst as well as preparation method and application thereof

    CN117802528A