Molybdenum-based catalyst and preparation method and application thereof
By introducing nickel elemental materials and nickel-molybdenum alloys into molybdenum-based catalysts, combined with heat treatment technology of carbon sources and reducing metals, the problems of improving activity and safety hazards of molybdenum-based catalysts are solved, and efficient catalytic effect of electrolyzed water hydrogen production is achieved.
Patent Information
- Application Number
- CN202411572161.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-06
AI Technical Summary
The catalytic activity of existing molybdenum-based catalysts needs to be improved, and there are safety hazards in the production process, especially leakage problems during hydrogen reduction.
Nickel elemental and/or nickel-molybdenum alloys are used as active components, combined with carbon source and reducing metals, and molybdenum-based catalysts are prepared in a protective atmosphere through specific heat treatment steps to avoid the use of hydrogen, improve catalytic activity and reduce safety hazards.
It achieves high-efficiency hydrogen evolution performance with catalytic activity similar to hydrogen reduction treatment, while avoiding safety hazards caused by hydrogen leakage, and is suitable for industrial production.
Smart Images

Figure CN119061429A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of catalytic materials, and specifically relates to a molybdenum-based catalyst and a preparation method and application thereof. Background Art
[0002] At present, the research on catalysts for hydrogen production by water electrolysis mainly focuses on precious metal catalysts, non-precious metal catalysts and composite catalysts. Precious metal catalysts such as platinum and palladium have good catalytic activity, but their high cost limits their popularity in large-scale applications. Non-precious metal catalysts such as transition metal compounds and carbon-based materials have lower costs and higher catalytic activity. At present, molybdenum-based catalysts show excellent catalytic activity and have the potential to replace platinum-carbon as hydrogen evolution catalysts.
[0003] In the prior art, the general steps of the preparation method of molybdenum-based catalysts include: first synthesizing a molybdate precursor by a hydrothermal method, and then performing a reduction treatment to obtain a molybdenum-based catalyst, wherein the reduction step is mostly carried out using hydrogen or other reducing substances. However, the process of hydrogen reduction involves hydrogen management and leakage issues, which poses a great safety hazard, thus limiting the industrial preparation of catalysts; if other reducing substances are used for reduction, the catalytic activity of the resulting catalyst is low and needs to be further improved. Summary of the invention Therefore, the technical problem to be solved by the present application is to overcome the defects in the prior art such as the need to further improve the activity of the molybdenum-based catalyst and / or the existence of potential safety hazards in production, thereby providing a molybdenum-based catalyst and its preparation method and application.
[0004] To this end, this application provides the following technical solutions: According to one aspect of the present application, a molybdenum-based catalyst is provided, comprising a substrate, and an active component supported on the substrate. Wherein, the active component includes molybdenum dioxide and also includes nickel and / or nickel-molybdenum alloy; The active component has a needle-like, rod-like or blade-like shape; and a size of the active component is nanometer-level or micrometer-level.
[0005] In some optional embodiments, the substrate carries a reducing metal oxide and / or a reducing metal.
[0006] In some optional embodiments, the substrate comprises a nickel-containing material, an iron-containing material, or a carbon-containing material, preferably nickel foam, nickel mesh, nickel sheet, nickel felt, iron foam, iron mesh, iron sheet, or carbon mesh, carbon cloth.
[0007] According to another aspect of the present application, there is provided a method for preparing a molybdenum-based catalyst, comprising the following steps: S1, loading a molybdenum-containing metal component on a substrate under heating conditions to obtain a precursor; wherein the heating temperature is 70-200° C. and the heating time is 1-48 hours; As an example, the heating temperature is 70°C, 80°C, 100°C, 130°C, 150°C, 170°C, 200°C, or within the range of any of the above values; the heating time is 1h, 5h, 10h, 15h, 20h, 24h, 26h, 48h, or within the range of any of the above values; S2, further comprising performing at least one of the following (1)-(3): (1) introducing a carbon source during the process of loading a molybdenum-containing metal component on a substrate; (2) Introducing a carbon source onto the surface of the precursor; (3) applying a reducing metal to the surface of the precursor; S3, heat treatment under protective atmosphere or vacuum conditions; It should be noted that the expressions S1, S2 and S3 in the preparation steps are only for the convenience of describing the preparation steps and do not represent the execution order between the steps.
[0008] In the present application, it is preferred that any two of (1)-(3) are executed in S2, and more preferably, all three are executed.
[0009] In some optional embodiments, in step S1, the heating temperature is 80-150° C., and the heating time is 5-24 h; And / or, in step S3, the heat treatment temperature is 450-900°C and the heat treatment time is 1s-2h. It should be noted that if the heat treatment time is too short, a device with particularly fast heating is required, for example, a Joule heating furnace is required if the heat treatment time is 1s.
[0010] As an example, the heat treatment temperature is 450°C, 500°C, 600°C, 700°C, 800°C, 900°C, or within the range of any of the above values; the heat treatment time is 1s, 30s, 5min, 30min, 1h, 1.5h, 2h, or within the range of any of the above values.
[0011] In the present application, the heat treatment in step S3 can be performed in one step or in multiple stages. When only item (1) is performed in S2, the heat treatment needs to be completed in one step, otherwise it will affect the activity of the catalyst.
[0012] In some optional embodiments, if one or more of items (1) and (2) in S2 are performed, the heat treatment includes the following steps: The temperature is raised to 400-1000° C., preferably 500° C., at a heating rate of 0.01-20° C. / min, preferably 10° C. / min, and maintained for 1 min-2 h, preferably 50 min-2 h.
[0013] In some optional embodiments, in (1) of the above step S2, a carbon source is introduced during the process of loading a molybdenum-containing metal component on a substrate, comprising the following steps: mixing a molybdenum source, a carbon source and a solvent to obtain a mixed solution A, immersing the substrate in the mixed solution A, soaking, and reacting under heating conditions to obtain a precursor.
[0014] In some optional embodiments, in step (2) of step S2 above, introducing a carbon source onto the surface of the precursor comprises: The precursor is immersed in a carbon source solution and dried.
[0015] In some optional embodiments, in step (3) of step S2 above, applying a reducing metal on the surface of the precursor comprises: The precursor is covered and encapsulated with a reducing metal.
[0016] In the present application, the reducing metal may be reducing metal particles or reducing metal powder, etc. In order to increase the contact area between the reducing metal and the precursor, reducing metal powder is preferred.
[0017] In some optional embodiments, if (1) introducing a carbon source during the process of loading the molybdenum-containing metal component on the substrate is not performed, loading the molybdenum-containing metal component on the substrate includes: A molybdenum source is mixed with a solvent to obtain a mixed solution B, and a substrate is immersed in the mixed solution B for soaking and reacting under heating conditions to obtain a precursor.
[0018] In some optional embodiments, the mixed solution A and / or the mixed solution B also includes a nickel source.
[0019] In some optional embodiments, the method for preparing the molybdenum-based catalyst satisfies at least one of the following (a)-(j): (a) The content of molybdenum source in the mixed solution A is 10-35 g / L; preferably 12-35 g / L; (b) The content of the carbon source in the mixed solution A is 0.1-18 g / L; preferably 3-18 g / L; (c) the content of nickel source in the mixed solution A is 0-40 g / L; (d) The content of molybdenum source in the mixed solution B is 10-35 g / L, preferably 12 g / L; (e) the content of nickel source in the mixed solution B is 1-40 g / L; (f) the carbon source content in the carbon source solution is 0.1-18 g / L; preferably 1-4 g / L; (g) The solvent of the mixed solution A and the mixed solution B includes water, and independently includes at least one of an alcohol solvent, hydrogen peroxide, and ammonium fluoride; in the present application, the use of ammonium fluoride is beneficial to the loading of the components; (h) the reducing metal comprises at least one of aluminum, magnesium and zinc; (i) The substrate comprises nickel foam, iron foam or carbon cloth; (j) The soaking time is 0-5h; as an example, the soaking time is 1min, 5min, 20min, 0.5h, 1h, 1.5h, 2h, 3h, 4h, 5h, or any range thereof; the soaking temperature is room temperature, for example, 25°C; in some optional embodiments, an oscillation treatment may be performed during the soaking process, and the oscillation frequency is 50-200rpm.
[0020] In the present application, the molybdenum source is conventional in the field, including but not limited to at least one of ammonium molybdate, molybdenum trioxide, and molybdenum powder.
[0021] In the present application, the nickel source is a soluble salt containing nickel, including but not limited to at least one of nickel nitrate, nickel sulfate, and nickel chloride.
[0022] In the present application, the carbon source is conventional in the art and can be a carbon-containing organic matter, including but not limited to at least one of glucose, carboxymethyl cellulose, polyvinyl pyrrolidone, p-phenylenediamine, amino acids, sodium alginate, sucrose, and the like.
[0023] In the present application, the alcohol solvent is conventional in the field, including but not limited to at least one of methanol, ethanol, isopropanol, etc.
[0024] In the present application, the protective atmosphere is a nitrogen atmosphere or an inert gas atmosphere, such as an argon atmosphere.
[0025] According to another aspect of the present application, there is provided an application of the above-mentioned molybdenum-based catalyst or the molybdenum-based catalyst prepared by the above-mentioned preparation method in hydrogen production by electrolysis of water.
[0026] The technical solution of this application has the following advantages: The molybdenum-based catalyst provided by the present application comprises a substrate, and an active component loaded on the substrate, wherein the active component comprises molybdenum dioxide, and also comprises nickel element and / or nickel-molybdenum alloy; or, the substrate is loaded with reducing metal oxide and / or reducing metal; the morphology of the active component is needle-shaped, rod-shaped or blade-shaped; the size of the active component is nanometer-scale or micrometer-scale. The molybdenum-based catalyst provided by the present application has a catalytic activity for hydrogen production by electrolysis of water that is much higher than similar catalysts obtained by reduction treatment using other reducing substances in the prior art, and is close to the catalytic activity of catalysts obtained by reduction treatment using hydrogen, avoiding the safety hazard caused by hydrogen leakage during the reduction treatment, and is conducive to the industrial production and application of the catalyst.
[0027] The preparation method of the molybdenum-based catalyst provided in the present application can reduce the catalyst in the absence of hydrogen by introducing a carbon source or a reducing metal, which can not only maintain the hierarchical structure morphology before the heat treatment, but also promote the reduction of molybdate to conductive molybdenum dioxide, thereby promoting material transport and charge transfer in the large current catalytic process, and achieving efficient hydrogen evolution catalytic activity. At the same time, this method also avoids the safety hazards caused by hydrogen leakage during the heat treatment process, which is beneficial to the industrial production and application of the catalyst.
[0028] The preparation method of the molybdenum-based catalyst provided in the present application can better dissolve raw materials such as molybdenum source, nickel source and / or carbon source by limiting the solvent in the mixed solution A and / or the mixed solution B, thereby facilitating the heating reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0030] Figure 1 is the test polarization curve of the platinum-based catalyst provided in Example 1 of the present application; Figure 2 is the test polarization curve of the platinum-based catalyst provided in Example 2 of the present application; Figure 3 is a scanning electron microscope image of the platinum-based catalyst provided in Example 2 of the present application; Figure 4 is the test polarization curve of the platinum-based catalyst provided in Example 3 of the present application; Figure 5 is the test polarization curve of the platinum-based catalyst provided in Example 4 of the present application; Figure 6 is the test polarization curve of the platinum-based catalyst provided in Example 5 of the present application; Figure 7 is the test polarization curve of the platinum-based catalyst provided in Example 6 of the present application; Figure 8 is the test polarization curve of the platinum-based catalyst provided in Example 7 of the present application; Fig. 9 is a scanning electron microscope image of the platinum-based catalyst provided in Example 7 of the present application; Fig.10 is the test polarization curve of the platinum-based catalyst provided in Example 8 of the present application; Fig.11 is the test polarization curve of the platinum-based catalyst provided in Example 9 of the present application; Fig.12 is a scanning electron microscope image of the platinum-based catalyst provided in Example 9 of the present application; Fig.13 is the test polarization curve of the platinum-based catalyst provided in Example 10 of the present application; Fig.14 is a scanning electron microscope image of the platinum-based catalyst provided in Example 10 of the present application; Fig.15 is the test polarization curve of the platinum-based catalyst provided in Example 11 of the present application; Fig.16 is a scanning electron microscope image of the platinum-based catalyst provided in Example 11 of the present application; Fig.17 is the test polarization curve of the platinum-based catalyst provided in Example 12 of the present application; Fig.18 is a scanning electron microscope image of the platinum-based catalyst provided in Example 12 of the present application; Fig.19 is the test polarization curve of the platinum-based catalyst provided in Example 13 of the present application; Fig. 20 is the XRD spectrum of the platinum-based catalyst provided in Example 13 of the present application; Fig.21 is a scanning electron microscope image of the platinum-based catalyst provided in Example 13 of the present application; Fig. 22 is the test polarization curve of the platinum-based catalyst provided in Example 14 of the present application; Fig.23 is the test polarization curve of the platinum-based catalyst provided in Example 15 of the present application; Fig.24 is the test polarization curve of the platinum-based catalyst provided in Example 16 of the present application; Fig.25is a scanning electron microscope image of the platinum-based catalyst provided in Example 16 of the present application; Fig.26 is the XRD spectrum of the platinum-based catalyst provided in Example 16 of the present application; Fig. 27 is the test polarization curve of the catalyst provided in Comparative Example 1 of the present application; Fig.28 is a scanning electron microscope image of the catalyst provided in Comparative Example 1 of the present application; Fig.29 is the test polarization curve of the catalyst provided in Comparative Example 2 of the present application; Fig.30 is a scanning electron microscope image of the catalyst provided in Comparative Example 2 of the present application; Fig.31 is the XRD spectrum of the catalyst provided in Comparative Example 2 of the present application; Fig.32 is the test polarization curve of the catalyst provided in Comparative Example 3 of the present application; Fig.33 This is the test polarization curve of the catalyst provided in Comparative Example 4 of the present application. DETAILED DESCRIPTION
[0031] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.
[0032] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0033] Example 1 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, polyvinyl pyrrolidone (Aladdin, molecular weight 10000) and water are mixed to obtain a mixed solution, in which the mass concentration of ammonium molybdate is 33 g / L and the mass concentration of polyvinyl pyrrolidone is 6 g / L.
[0034] (2) The nickel foam and the mixed solution were placed on an oscillator, and the nickel foam (thickness 1 mm, 100 PPI) was immersed in the mixed solution and oscillated for 2 h at a frequency of 150 rpm to obtain a white-green suspension; wherein the immersion and oscillation temperature was 25°C.
[0035] (3) The nickel foam and the white-green suspension were subjected to a hydrothermal reaction at 150°C for 6 hours to obtain a catalyst precursor; the temperature was then increased to 500°C at a heating rate of 10°C / min, and the temperature was maintained at 500°C for 20 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere was pure argon.
[0036] Example 2 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, carboxymethyl cellulose and water are mixed to obtain a mixed solution, wherein the mass concentration of ammonium molybdate in the mixed solution is 33 g / L, and the mass concentration of carboxymethyl cellulose is 6 g / L.
[0037] (2) The nickel foam and the mixed solution are placed in an oscillator, and the nickel foam is immersed in the mixed solution and oscillated for 2 hours at a frequency of 150 rpm to obtain a white-green suspension; wherein the immersion and oscillation temperature is 25°C.
[0038] (3) The nickel foam and the white-green suspension were subjected to a hydrothermal reaction at 150°C for 6 hours to obtain a catalyst precursor; the catalyst precursor was covered with Mg powder and wrapped with aluminum foil, and then heated to 600°C at a heating rate of 10°C / min, and maintained at 600°C for heat treatment for 30 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere was pure argon.
[0039] Example 3 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, p-phenylenediamine and water are mixed to obtain a mixed solution, wherein the mass concentration of ammonium molybdate in the mixed solution is 33 g / L, and the mass concentration of p-phenylenediamine is 6 g / L.
[0040] (2) The nickel foam and the mixed solution are placed in an oscillator, and the nickel foam is immersed in the mixed solution and oscillated for 2 hours at a frequency of 150 rpm to obtain a white-green suspension; wherein the immersion and oscillation temperature is 25°C.
[0041] (3) The nickel foam and the white-green suspension were subjected to a hydrothermal reaction at 150°C for 6 hours to obtain a catalyst precursor; the catalyst precursor was soaked in a 2 g / L glucose solution for several minutes and then dried, and then heated to 700°C at a heating rate of 10°C / min, and maintained at 700°C for heat treatment for 2 hours to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere was pure argon.
[0042] Example 4 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, polyvinyl pyrrolidone (Aladdin, molecular weight 10000) and water were mixed to obtain a mixed solution, in which the mass concentration of ammonium molybdate was 33 g / L and the mass concentration of polyvinyl pyrrolidone was 3 g / L.
[0043] (2) The nickel foam and the mixed solution are placed in an oscillator, and the nickel foam is immersed in the mixed solution and oscillated for 2 hours at a frequency of 150 rpm to obtain a white-green suspension; wherein the immersion and oscillation temperature is 25°C.
[0044] (3) The nickel foam and the white-green suspension were subjected to a hydrothermal reaction at 150°C for 6 hours to obtain a catalyst precursor; the catalyst precursor was soaked in a 2 g / L glucose solution for several minutes and then dried, and then heated to 600°C at a heating rate of 10°C / min, and maintained at 600°C for heat treatment for 1 hour to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere was pure argon.
[0045] Example 5 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, polyvinyl pyrrolidone (Aladdin, molecular weight 10000) and water are mixed to obtain a mixed solution, in which the mass concentration of ammonium molybdate is 33 g / L and the mass concentration of polyvinyl pyrrolidone is 6 g / L.
[0046] (2) The nickel foam and the mixed solution are placed in an oscillator, and the nickel foam is immersed in the mixed solution and oscillated for 2 hours at a frequency of 150 rpm to obtain a white-green suspension; wherein the immersion and oscillation temperature is 25°C.
[0047] (3) The nickel foam and the white-green suspension were subjected to a hydrothermal reaction at 150°C for 6 hours to obtain a catalyst precursor; the catalyst precursor was soaked in 2 g / L polyvinyl pyrrolidone for several minutes and then dried, and then heated to 500°C at a heating rate of 10°C / min, and maintained at 500°C for 20 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere was pure argon.
[0048] Example 6 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of ammonium fluoride is 6 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0049] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0050] (3) The catalyst precursor was immersed in a 3 g / L sucrose solution for several minutes and then dried. The temperature was then raised to 850° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 seconds to obtain a molybdenum-based catalyst. The heat treatment atmosphere was a vacuum.
[0051] Example 7 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of ammonium fluoride is 6 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0052] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0053] (3) The catalyst precursor was immersed in a 3 g / L p-phenylenediamine solution for several minutes and then dried. The catalyst precursor was then heated to 750° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 minutes to obtain a molybdenum-based catalyst. The heat treatment atmosphere was a vacuum.
[0054] Example 8 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of ammonium fluoride is 6 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0055] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0056] (3) The catalyst precursor was immersed in a 2 g / L polyvinyl alcohol (Aladdin, molecular weight 10,000) solution for several minutes and then dried. The catalyst precursor was then heated to 850° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 minutes to obtain a molybdenum-based catalyst. The heat treatment atmosphere was a vacuum.
[0057] Example 9 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of ammonium fluoride is 6 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0058] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0059] (3) The catalyst precursor was immersed in a 1 g / L polyvinyl pyrrolidone (Aladdin, molecular weight 10,000) solution for several minutes, dried, covered with reducing metal Al powder and wrapped with aluminum foil, and then heated to 600°C in a Joule heating furnace at a rate of 1 second and heat treated for 10 min to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere was a vacuum.
[0060] Example 10 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, p-phenylenediamine, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of p-phenylenediamine is 6 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0061] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0062] (3) The catalyst precursor was immersed in a 1 g / L glucose solution for several minutes and then dried, and then heat treated in a Joule heating furnace at a temperature of 500° C. for 5 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere is a vacuum.
[0063] Embodiment 11 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, polyvinyl pyrrolidone (Aladdin, molecular weight 10000), ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of polyvinyl pyrrolidone is 6 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0064] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0065] (3) The catalyst precursor is immersed in 1 g / L glucose solution for several minutes, dried, covered with reducing metal Zn powder and wrapped with aluminum foil, and then heated to 500° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere is a vacuum.
[0066] Example 12 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, polyvinyl pyrrolidone (Aladdin, molecular weight 10000), ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of polyvinyl pyrrolidone is 12 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0067] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0068] (3) The catalyst precursor is immersed in a 1 g / L p-phenylenediamine solution for several minutes and then dried. The catalyst precursor is then heated to 500° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 minutes to obtain a molybdenum-based catalyst. The heat treatment atmosphere is a vacuum.
[0069] Example 13 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, glucose, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of glucose is 12 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0070] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0071] (3) The catalyst precursor is immersed in 3 g / L sodium alginate solution for several minutes, dried, covered with reducing metal Al powder and wrapped with aluminum foil, and then heated to 500° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere is a vacuum.
[0072] Embodiment 14 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, polyvinyl pyrrolidone (Aladdin, molecular weight 10000), ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of polyvinyl pyrrolidone is 18 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0073] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0074] (3) The catalyst precursor was immersed in a 4 g / L glucose solution for several minutes and then dried. The catalyst precursor was then heated to 500° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 minutes to obtain a molybdenum-based catalyst. The heat treatment atmosphere was a vacuum.
[0075] Embodiment 15 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, nickel nitrate and a sucrose aqueous solution are mixed to obtain a mixed solution, wherein the mass concentration of ammonium molybdate is 30 g / L, the mass concentration of nickel nitrate is 30 g / L, and the mass concentration of sucrose is 9 g / L.
[0076] (2) The nickel foam and the mixed solution are placed in a reactor and subjected to a hydrothermal reaction at 150° C. for 6 h to obtain a catalyst precursor.
[0077] (3) The catalyst precursor is soaked in 1 g / L glucose solution, dried, covered with reducing metal Mg powder and wrapped with aluminum foil, and then heat-treated in a Joule heating furnace at 500° C. for 5 min to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere is a vacuum.
[0078] Example 16 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, nickel nitrate and water are mixed to obtain a mixed solution, wherein the mass concentration of ammonium molybdate in the mixed solution is 30 g / L, and the mass concentration of nickel nitrate is 30 g / L.
[0079] (2) The nickel foam and the mixed solution are placed in a reactor and subjected to a hydrothermal reaction at 150° C. for 6 h to obtain a catalyst precursor.
[0080] (3) The catalyst precursor is covered with reducing metal Mg powder and wrapped with aluminum foil, and then heated to 500°C in a tubular furnace at a heating rate of 5°C / min, and maintained at this temperature for 20 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere is pure argon.
[0081] Embodiment 17 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, nickel nitrate, polyvinyl pyrrolidone and water are mixed to obtain a mixed solution, wherein the mass concentration of ammonium molybdate in the mixed solution is 35 g / L, the mass concentration of nickel nitrate is 30 g / L, and the mass concentration of polyvinyl pyrrolidone is 6 g / L.
[0082] (2) The foamed iron and the mixed solution are placed in an oscillator, and the foamed iron is immersed in the mixed solution and oscillated for 2 h at a frequency of 150 rpm to obtain a white-green suspension; wherein the immersion and oscillation temperature is 25°C.
[0083] (3) The foamed iron and the white-green suspension were subjected to a hydrothermal reaction at 140°C for 5 hours to obtain a catalyst precursor; the temperature was then increased to 500°C at a heating rate of 10°C / min, and the temperature was maintained at 500°C for 20 minutes to obtain a molybdenum-based catalyst; wherein the heat treatment atmosphere was pure argon.
[0084] Embodiment 18 This embodiment provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, polyvinyl pyrrolidone, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of polyvinyl pyrrolidone is 12 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0085] (2) The carbon cloth and the mixed solution were placed in a glass vial and reacted at 80°C. The liquid level was kept constant during the reaction. The reaction lasted for 24 hours to obtain a catalyst precursor.
[0086] (3) The catalyst precursor is immersed in a 1 g / L p-phenylenediamine solution for several minutes and then dried. The catalyst precursor is then heated to 500° C. in a Joule heating furnace at a rate of 1 second and heat treated for 5 minutes to obtain a molybdenum-based catalyst. The heat treatment atmosphere is a vacuum.
[0087] Comparative Example 1 This comparative example provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0088] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0089] (3) Wrapping the catalyst precursor with aluminum foil, heating it to 500° C. in a Joule heating furnace for 1 second, and calcining it for 3 minutes to obtain a molybdenum-based catalyst; wherein the treatment atmosphere is a vacuum.
[0090] Comparative Example 2 This comparative example provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, nickel nitrate and water are mixed to obtain a mixed solution, wherein the mass concentration of ammonium molybdate in the mixed solution is 30 g / L, and the mass concentration of nickel nitrate is 30 g / L.
[0091] (2) The nickel foam and the mixed solution are placed in a reactor and subjected to a hydrothermal reaction at 150° C. for 6 h to obtain a catalyst precursor.
[0092] (3) Wrapping the catalyst precursor with aluminum foil, heating it to 500°C in a tubular furnace at a heating rate of 5°C / min, and maintaining the temperature for calcination for 20 minutes to obtain a molybdenum-based catalyst; wherein the treatment atmosphere is pure argon.
[0093] Comparative Example 3 This comparative example provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Ammonium molybdate, polyvinyl pyrrolidone (Aladdin, molecular weight 10000) and water are mixed to obtain a mixed solution, in which the mass concentration of ammonium molybdate is 33 g / L and the mass concentration of polyvinyl pyrrolidone is 6 g / L.
[0094] (2) The nickel foam and the mixed solution were placed on an oscillator, and the nickel foam (thickness 1 mm, 100 PPI) was immersed in the mixed solution and oscillated for 2 h at a frequency of 150 rpm to obtain a white-green suspension; wherein the immersion and oscillation temperature was 25°C.
[0095] (3) The nickel foam and the white-green suspension were subjected to a hydrothermal reaction at 150° C. for 6 hours to obtain a catalyst precursor; the temperature was first kept constant at 250° C. for 1 hour, and then the temperature was increased to 500° C. and kept constant for 20 minutes; the heat treatment atmosphere was pure argon.
[0096] Comparative Example 4 This comparative example provides a method for preparing a molybdenum-based catalyst, and the specific steps and operating parameters are as follows: (1) Molybdenum trioxide, nickel nitrate, hydrogen peroxide, p-phenylenediamine, ammonium fluoride, ethanol and water are mixed to obtain a mixed solution, wherein the mass concentration of molybdenum trioxide in the mixed solution is 12 g / L, the mass concentration of nickel nitrate is 40 g / L, the mass concentration of p-phenylenediamine is 6 g / L, the mass concentration of ammonium fluoride is 3 g / L, the total volume of hydrogen peroxide is 5 ml, the total volume of ethanol is 6 ml, and the total volume of water is 7 ml.
[0097] (2) Place the nickel foam and the mixed solution in a glass vial and react at 80°C while keeping the liquid level constant. The reaction is continued for 24 hours to obtain a catalyst precursor.
[0098] (3) The catalyst precursor was soaked in 1g / L glucose solution for several minutes, dried and wrapped with aluminum foil, and then heated in sections in a tubular furnace to obtain a molybdenum-based catalyst. The temperature was first kept constant at 250°C for 1 hour, and then the temperature was increased to 500°C and kept constant for 20 minutes to obtain the molybdenum-based catalyst; the heat treatment atmosphere was vacuum.
[0099] Table 1
[0100] Note: “ / ” represents that the corresponding component was not introduced.
[0101] Test Case The catalysts provided in each embodiment and comparative example of the present application were subjected to XRD, SEM and catalytic performance tests, and the specific test methods are as follows: 1. XRD uses Bruker D8 advance with a scanning range of 5-80 degrees; 2. Scanning electron microscope test uses Zeiss electron microscope (Gemini 450 microscope system); 3. Catalytic performance The three-electrode test method was adopted, with the catalyst as the cathode (the catalyst was from each embodiment and comparative example), the counter electrode being a graphite sheet, and the reference electrode being a saturated calomel electrode. The measurement was carried out in a glass electrolytic cell, and the electrolyte was a potassium hydroxide solution with a molar concentration of 1 mol / L. The linear sweep voltammetry was carried out from 0 V to -0.4 V, with a scan rate of 5 mV / s.
[0102] Specific test results are as follows Figure 1-Figure 33 As shown, Figure 1 , 2, 4, 5, 6, 7, 8, 10, 11, 13, 15, 17, 19, 22, 23, 24, 27, 29, 32, 33 are the test polarization curves of Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16 and Comparative Examples 1, 2, 3, 4 respectively; Figure 3 , 9, 12, 14, 16, 18, 21, 25, 28, 30 are scanning electron microscope images of Examples 2, 7, 9, 10, 11, 12, 13, 16 and Comparative Examples 1 and 2; Fig. 20 , 26, 31 are XRD diagrams of Examples 13, 16 and Comparative Example 2. From the polarization curves, it can be seen that Examples 1-16 have a high 2 The overpotential at a current density of is significantly lower than that of Comparative Examples 1 and 2 without heat treatment; and the performance is better than that of Comparative Examples 3 and 4 obtained by segmented reduction. In addition, it can be seen from the scanning electron microscope image that the various reduction treatment methods used in this application can still well maintain the nano-morphology of the catalyst hierarchical structure, thereby ensuring efficient material transfer and charge transfer under high current density. From the XRD diagram, it can be seen that, in combination with a variety of heat treatment methods, Example 13 can be completely reduced to a heterogeneous structure of molybdenum dioxide and nickel-molybdenum alloy. Although Example 16 is not completely reduced, it still has obvious molybdenum dioxide phase and metal phase. For Comparative Example 2, there is no obvious reduction effect.
[0103] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A platinum-based catalyst, characterized in that comprising a substrate, and an active component loaded on the substrate, Wherein, the active component includes molybdenum dioxide and also includes nickel and / or nickel-molybdenum alloy; The active component has a needle-like, rod-like or blade-like shape; and a size of the active component is nanometer-level or micrometer-level.
2. The platinum-based catalyst according to claim 1, characterized in that The substrate supports reducing metal oxides and / or reducing metals.
3. The platinum-based catalyst according to claim 1 or 2, characterized in that The substrate includes a nickel-containing material, an iron-containing material, or a carbon-containing material.
4. A method for preparing a molybdenum-based catalyst, characterized in that: The steps include: S1, under heating conditions, loading a molybdenum-containing metal component on a substrate to obtain a precursor; wherein the heating temperature is 70-200° C. and the heating time is 1-48 hours; S2, further comprising performing at least one of the following (1)-(3): (1) introducing a carbon source during the process of loading a molybdenum-containing metal component on a substrate; (2) Introducing a carbon source onto the surface of the precursor; (3) applying a reducing metal to the surface of the precursor; S3, heat treatment is carried out under protective atmosphere or vacuum conditions.
5. The method for preparing a platinum-based catalyst according to claim 4, characterized in that: In step S1, the heating temperature is 80-150°C and the heating time is 5-24h; And / or, in step S3, the heat treatment temperature is 450-900° C., and the heat treatment time is 1 s-2 h.
6. The method for preparing a platinum-based catalyst according to claim 4, characterized in that: If one or more of items (1) and (2) in S2 are performed, the heat treatment includes the following steps: Raise the temperature to 400-1000°C at a rate of 0.01-20°C / min and maintain for 1 min-2 h.
7. The method for preparing a platinum-based catalyst according to claim 4, characterized in that: (1), introducing a carbon source during the process of loading a molybdenum-containing metal component on a substrate comprises the following steps: mixing a molybdenum source, a carbon source and a solvent to obtain a mixed solution A, immersing the substrate in the mixed solution A, and reacting under heating conditions to obtain a precursor.
8. The method for preparing a platinum-based catalyst according to claim 4, characterized in that: (2) Introducing a carbon source on the surface of the precursor includes: The precursor is immersed in a carbon source solution and dried.
9. The method for preparing a platinum-based catalyst according to claim 4, characterized in that: (3), applying a reducing metal to the surface of the precursor includes: The precursor is covered and encapsulated with a reducing metal.
10. The method for preparing a platinum-based catalyst according to claim 4, characterized in that: If (1) introducing a carbon source during the process of loading the molybdenum-containing metal component on the substrate is not performed, the process of loading the molybdenum-containing metal component on the substrate includes: A molybdenum source is mixed with a solvent to obtain a mixed solution B, and a substrate is immersed in the mixed solution B for soaking and reacting under heating conditions to obtain a precursor.
11. The method for preparing a platinum-based catalyst according to claim 7 or 10, characterized in that: The mixed solution A and / or the mixed solution B also includes a nickel source.
12. The method for preparing a molybdenum-based catalyst according to claim 11, characterized in that: Satisfy at least one of the following (a)-(j): (a) the content of molybdenum source in the mixed solution A is 10-35 g / L; (b) the content of the carbon source in the mixed solution A is 0.1-18 g / L; (c) the content of nickel source in the mixed solution A is 0-40 g / L; (d) the content of molybdenum source in the mixed solution B is 10-35 g / L; (e) the content of nickel source in the mixed solution B is 1-40 g / L; (f) the carbon source content in the carbon source solution is 0.1-18 g / L; (g) the solvent of the mixed solution A and the mixed solution B includes water, and independently includes at least one of an alcohol solvent, hydrogen peroxide, and ammonium fluoride; (h) the reducing metal comprises at least one of aluminum, magnesium and zinc; (i) The substrate comprises nickel foam, iron foam or carbon cloth; (j) The soaking time is 0-5h.
13. Use of the molybdenum-based catalyst according to any one of claims 1 to 3 or the molybdenum-based catalyst prepared by the preparation method according to any one of claims 4 to 12 in hydrogen production by electrolysis of water.
Citation Information
Patent Citations
Mesopore carbon load nickel hydrogenation catalyst and preparation method thereof
CN101693201A
Preparation method of carbon-loaded Ru base catalyst by carbon thermal reduction
CN106622218A
Titanium dioxide loaded nanoscale Ru metal stub composite material, and preparation method and application thereof
CN111359607A
High-efficiency bimetallic nickel molybdenum selenide electro-catalytic material and preparation method thereof
CN111495395A
Preparation method of nickel-molybdenum carbide electrocatalyst
CN113846343A
Cited By
Hydrogen production catalyst as well as preparation method and application thereof
CN120272954A