Nickel-cobalt alloy with multi-gradient structure and preparation method of nickel-cobalt alloy

The formation of multiple gradient structure nickel-cobalt alloys through electrochemical deposition method solves the problem of strength and plasticity balance in extreme operating conditions, achieves good service performance in high temperature, high pressure and high speed friction environments, and broadens the application scope.

CN119061447APending Publication Date: 2024-12-03NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411242699.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional homogeneous structure nickel-cobalt alloy coatings are difficult to meet service performance requirements in harsh environments such as high temperature, high pressure and high speed friction, and are difficult to balance strength and plasticity, making it difficult to last service under extreme operating conditions.

Method used

By using electrochemical deposition, the gradual increase of current density, cobalt salt concentration and saccharin sodium concentration, combined with temperature adjustment, a multi-gradient structure nickel-cobalt alloy with grain size gradient, component gradient and phase structure gradient is formed to achieve grain grains. The transition from the micrometer to the nanometer scale, the gradient changes in cobalt content and phase structure.

Benefits of technology

It improves the strength, hardness and plastic deformation capabilities of the coating, enhances the load-bearing capacity under high loads, and broadens the application range of nickel-based alloys in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061447A_ABST
    Figure CN119061447A_ABST
Patent Text Reader

Abstract

The invention relates to a nickel-cobalt alloy with a multi-gradient structure and a preparation method of the nickel-cobalt alloy. Comprising the following steps that electrochemical deposition is adopted, nickel serves as a consumable anode, the current density is controlled to be gradually increased, the concentration of cobalt salt in electroplating liquid is controlled to be gradually increased along with time, the concentration of saccharin sodium salt is controlled to be gradually increased, and the temperature of the electroplating liquid is controlled; and depositing under the action of direct current to form the nickel-cobalt alloy with the triple gradient structure, which is compounded with the grain size gradient, the component gradient and the phase structure gradient at the same time. According to the gradient-structure nickel-cobalt alloy prepared through the method, the application range of the nickel-based alloy under the complex and severe service conditions can be further widened, and technical reserve is provided for future engineering application; the gradient-structure nickel-cobalt alloy can eliminate performance mutation caused by component change, the coupling effect of the multi-gradient structure is exerted, and therefore cooperative improvement of the multi-target performance of the whole material is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal materials, and in particular relates to a nickel-cobalt alloy with a multiple gradient structure and a preparation method thereof. Background Art

[0002] Nickel-cobalt alloys are widely used in advanced manufacturing, energy, electronics, aerospace and other fields due to their high strength, high wear resistance, good corrosion resistance, special electrocatalytic activity and excellent soft magnetic properties. They are important coating materials for surface protection of key components of high-end equipment. For example, in the inner bore of a gun barrel, nickel-cobalt plating can be used as a good substitute for traditional hard chrome plating, and it is more in line with the concept of green development than hard chrome plating that causes serious pollution.

[0003] Among the existing nickel-cobalt alloy coating preparation processes, the electrodeposition method stands out for its low cost and excellent coating uniformity. Its sample size is almost unlimited and its controllability is high, making the electrodeposition method widely used in high-precision machining and surface corrosion protection. However, in the field of military equipment and engine parts manufacturing, the inner bore of the gun barrel, the engine piston and other parts need to serve in harsh and complex environments such as high temperature, high pressure and high-speed friction. The traditional homogeneous structure nickel-cobalt alloy coating is difficult to meet the service performance requirements under extreme working conditions due to its weak interface bonding and poor plasticity / toughness. For example, although the traditional homogeneous coarse-grained nickel-cobalt alloy has good plasticity / toughness, it has poor strength and low surface hardness, making it difficult to serve under conditions that require high load friction; while the homogeneous nanocrystalline nickel-cobalt alloy has high strength and hardness, it is brittle and easy to crack, and cannot effectively bear deformation under extreme working conditions. Therefore, how to ensure the plasticity and toughness of the material without sacrificing strength and hardness, this balance between strength and plasticity has long been the bottleneck that restricts the long-term service of materials under extreme working conditions.

[0004] At present, in response to the demand for new metal materials, gradient structures have been widely introduced into their design and development in order to achieve the versatility of the overall material. The microstructure, composition or atomic structure of the gradient material presents a gradient distribution in space, which enables the material to achieve simultaneous optimization and improvement of multiple properties. Patent documents CN104862748A, CN202010070014.6 and CN115449867A respectively disclose a grain-scale gradient metal nickel and a controllable preparation method thereof, a gradient structure nickel-tungsten alloy, a preparation method and a new layered structure and a preparation process of an electrodeposited single-phase composition gradient nanocrystalline iron-cobalt-nickel alloy. The introduction of gradient materials into nickel-cobalt alloy coatings is expected to simultaneously improve the strength and plasticity of the material, and achieve long-term good service of the material under extreme working conditions. Summary of the invention

[0005] The object of the present invention is to provide a nickel-cobalt alloy with a multiple gradient structure and a preparation method thereof.

[0006] The technical solution to achieve the purpose of the present invention is: a method for preparing a nickel-cobalt alloy with a multiple gradient structure, comprising the following steps: using electrochemical deposition, using nickel as a consumable anode, controlling the current density to gradually increase, controlling the cobalt salt concentration in the electroplating solution to gradually increase over time, controlling the concentration of saccharin sodium to gradually increase, and controlling the plating solution temperature, and depositing under the action of direct current to form a triple gradient structure nickel-cobalt alloy with a grain size gradient, a composition gradient and a phase structure gradient.

[0007] Furthermore, the plating solution used for electrochemical deposition includes nickel sulfate hexahydrate with a concentration of 100±10 g / L, sodium bromide with a concentration of 30±3 g / L, boric acid with a concentration of 30±3 g / L, and sodium dodecyl sulfate with a concentration of 0.3±0.03 g / L; the pH of the plating solution is adjusted to 4.5±0.1; and the temperature of the plating solution is 45-75°C.

[0008] Furthermore, the cathode is titanium, copper, copper alloy, steel or nickel.

[0009] Furthermore, the current density during deposition was increased from 30 mA / cm 2 Gradually increase to 50mA / cm 2 .

[0010] Furthermore, the cobalt salt is cobalt sulfate heptahydrate; during the deposition process, the concentration of cobalt sulfate heptahydrate is controlled to gradually increase from 0 g / L to 80 g / L.

[0011] Further, the concentration of saccharin sodium is controlled to gradually increase from 0.5 g / L to 5.5 g / L; specifically, the concentration of saccharin sodium is maintained at 0.5 g / L within 1 hour after the start of electrochemical deposition, and then the concentration of saccharin sodium is gradually increased from 0.5 g / L to 1.04 g / L within 1-1.5 hours, and then the concentration of saccharin sodium is gradually increased from 1.04 g / L to 1.69 g / L within 1 hour, and then the concentration of saccharin sodium is gradually increased from 1.69 g / L to 2.66 g / L within 1 hour, and then the concentration of saccharin sodium is gradually increased from 2.66 g / L to 3.92 g / L within 1 hour, and then the concentration of saccharin sodium is gradually increased from 3.92 g / L to 5.5 g / L within 1 hour, and finally the concentration of saccharin sodium is maintained at 5.5 g / L within the next 1.5 hours.

[0012] Furthermore, during the electrochemical deposition process, the temperature of the plating solution is controlled in the following manner:

[0013] Stage a: Control the temperature of the plating solution to 75°C within 1-1.5 hours after the start of electrochemical deposition;

[0014] Stage b: within 0.5-1h after the end of stage a, adjust the temperature of the plating solution to 64-66°C;

[0015] Stage c: Adjust the temperature of the plating solution to 59-61°C within 1-1.5 hours after the end of stage b;

[0016] Stage d: Keep the temperature of the plating solution at 59-61°C within 4-5 hours after the end of stage c;

[0017] Stage e: within 1-1.5 hours after the end of stage d, adjust the temperature of the plating solution to 49-51°C;

[0018] Stage f: Adjust the temperature to 44-46°C within 0.5-1.5 hours after the end of stage e;

[0019] The temperature in stages b, c, e and f is adjusted at a uniform speed.

[0020] Furthermore, the substrate is pretreated before deposition, specifically: mechanically polishing and surface degreasing the substrate;

[0021] Mechanical polishing specifically includes using 800#, 1000# and 1500# sandpaper to polish the surface of the substrate in sequence;

[0022] Surface degreasing is the process of cleaning the substrate surface with an organic solvent.

[0023] A multi-gradient structure nickel-cobalt alloy is prepared by the above method, wherein the grain size gradually transitions from micron-sized coarse grains to nano-sized grains along the deposition direction, the cobalt content gradually increases along the deposition direction, and the single-phase face-centered cubic structure gradually changes to a dual-phase structure in which face-centered cubic and close-packed hexagonal coexist.

[0024] Furthermore, the grain size of the gradient structured nickel-cobalt alloy is gradually refined from 10-20 μm to 20-40 nm;

[0025] The atomic percentage of cobalt in the gradient structure nickel-cobalt alloy ranges from 0 to 82%.

[0026] Compared with the prior art, the present invention has the following significant advantages:

[0027] The present invention provides a gradient structure nickel-cobalt alloy, a preparation method and a new gradient structure. By using electrochemical deposition technology, by regulating the current density, the addition rate of sodium saccharin and cobalt sulfate while depositing, a grain size gradient with a transition from micron-level coarse crystal to ultrafine crystal to nanocrystal, a composition gradient with a gradually changing cobalt content and a multiple gradient structure nickel-cobalt alloy transformed from FCC phase to FCC+HCP dual-phase structure can be prepared, and the corresponding gradient distribution form is precisely controllable. This is conducive to avoiding the sudden change of the metal properties of each component, thereby regulating the various properties of the overall material in a larger composition and scale space. Since the HCP structure on the surface has fewer slip systems and the grain size belongs to nanocrystals, it jointly increases the strength and hardness of the surface layer, so that the coating surface has good tribological properties; at the same time, the FCC structure and the larger grain size of the subsurface layer jointly ensure the plastic deformation ability of the material, so that the coating is not easy to crack and can effectively bear deformation under high load. The gradient structure nickel-cobalt alloy prepared by the above method can further broaden the application range of nickel-based alloys under complex and harsh service conditions such as high temperature, high pressure and high-speed friction environments, and provide technical reserves for future engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The cross-sectional microstructure morphology, cross-sectional phase distribution, cross-sectional element distribution and cross-sectional hardness value distribution of the electrochemically deposited gradient structure nickel-cobalt alloy sample I in Example 1;

[0029] Figure 2 The cross-sectional microstructure morphology, cross-sectional phase distribution, cross-sectional element distribution and cross-sectional hardness value distribution of the typical electrochemically deposited gradient structure nickel-cobalt alloy sample II in Example 2;

[0030] Figure 3 The cross-sectional microstructure morphology, cross-sectional phase distribution, cross-sectional element distribution and cross-sectional hardness value distribution of the typical electrochemically deposited gradient structure nickel-cobalt alloy sample III of Example 3;

[0031] Figure 4 The grain size distribution of the typical gradient structure nickel-cobalt alloy electrochemically deposited in Examples 1-3. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0033] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0034] Example 1

[0035] This embodiment provides a method for preparing a gradient structure nickel-cobalt alloy, which comprises the following steps:

[0036] (1) In this embodiment, a metal nickel plate with a purity of 99.6% is used as a consumable anode, and a metal copper plate is used as a cathode.

[0037] Prepare 1000ml of plating solution. The basic plating solution includes the following chemical reagents: NiSO4·6H2O: 100g / L, NaBr: 30g / L, H3BO3: 30g / L, C7H8NNaO5S: 0.5g / L, C 12 H 25 SO4Na: 0.3g / L. Weigh the above chemical reagents with a balance, dissolve them in ultrapure water in a 1000ml beaker, stir the solution with a magnetic stirrer until it is clear, adjust the pH value of the solution to 4.5±0.1 with dilute sulfuric acid solution or sodium hydroxide solution, and use a heating device to control the initial temperature of the plating solution to 75±1℃.

[0038] (2) Use computer to control current density and additive concentration:

[0039] Current density: During the entire electrochemical deposition process, the current density remained constant at 30 mA / cm 2 .

[0040] At the same time, the concentration of the additive saccharin sodium was regulated: the concentration of saccharin sodium was maintained at 0.5 g / L within 1 hour after the start of electrochemical deposition, and then the concentration of saccharin sodium gradually increased from 0.5 g / L to 1.04 g / L within 1-1.5 hours, and then the concentration of saccharin sodium gradually increased from 1.04 g / L to 1.69 g / L within 1 hour, and then the concentration of saccharin sodium gradually increased from 1.69 g / L to 2.66 g / L within 1 hour, and then the concentration of saccharin sodium gradually increased from 2.66 g / L to 3.92 g / L within 1 hour, and then the concentration of saccharin sodium gradually increased from 3.92 g / L to 5.5 g / L within 1 hour, and finally the concentration of saccharin sodium remained unchanged at 5.5 g / L within the next 1.5 hours.

[0041] At the same time, the concentration of the additive cobalt sulfate heptahydrate was regulated: the concentration of cobalt sulfate heptahydrate was maintained at 0 g / L within 1 hour after the start of electrochemical deposition, and then the concentration of cobalt sulfate heptahydrate was gradually increased from 0 g / L to 1 g / L within 0.5 hours, and then the concentration of cobalt sulfate heptahydrate was gradually increased from 1 g / L to 3.5 g / L within 1 hour, and then the concentration of cobalt sulfate heptahydrate was increased to 8.5 g / L within 5 hours, and then the concentration of cobalt sulfate heptahydrate was adjusted to 80 g / L within 1 hour, and finally the concentration of cobalt sulfate heptahydrate was kept unchanged at 80 g / L within the next 1.5 hours.

[0042] Simultaneously, the temperature of the plating solution is controlled in the following manner:

[0043] Stage a: controlling the temperature of the plating solution to 75°C within 1-1.5 hours after the start of electrochemical deposition;

[0044] Stage b: within 0.5-1h after the end of stage a, the temperature of the plating solution is adjusted to 64-66°C;

[0045] Stage c: within 1-1.5 hours after the end of stage b, the temperature of the plating solution is adjusted to 59-61°C;

[0046] Stage d: maintaining the temperature of the plating solution at 59-61° C. within 4-5 hours after the end of stage c;

[0047] Stage e: within 1-1.5 hours after the end of stage d, the temperature of the plating solution is adjusted to 49-51° C.;

[0048] Stage f: Adjust the temperature to 44-46°C within 0.5-1.5 hours after the end of stage e;

[0049] The temperature adjustment in the stages b, c, e and f is all uniform.

[0050] The gradient structure nickel-cobalt alloy sample I prepared in this embodiment is Figure 1 As shown in Figures ab, the grain size of sample I gradually refines from micrometer level to nanometer level, and there is no obvious macro interface. The coating quality is good without obvious microcracks.

[0051] Phase distribution reference of electrochemically deposited gradient structure nickel-cobalt alloy sample I Figure 1 As shown in c, it can be seen that from the matrix to the surface, the phase structure gradually changes from single-phase FCC to dual-phase FCC+HCP structure.

[0052] The cross-sectional distribution of cobalt content and nickel content of electrochemically deposited gradient structure nickel-cobalt alloy sample I is shown in Figure 2. Figure 1 As shown in Figure d, it can be seen that the cobalt content gradually increases from 0 at% to ~82 at%.

[0053] Reference for the cross-sectional hardness distribution of gradient structure nickel-cobalt alloy Figure 1 As shown in Fig. e, the hardness gradually increases from 2 GPa to 5.2 GPa, and then remains at around 5.2 GPa.

[0054] Example 2

[0055] This embodiment provides a method for preparing a gradient structure nickel-cobalt alloy, which comprises the following steps:

[0056] (1) In this embodiment, a metal nickel plate with a purity of 99.6% is used as a consumable anode, and a metal copper plate is used as a cathode.

[0057] Prepare 1000ml of plating solution. The basic plating solution includes the following chemical reagents: NiSO4·6H2O: 100g / L, NaBr: 30g / L, H3BO3: 30g / L, C7H8NNaO5S: 0.5g / L, C 12 H 25 SO4Na: 0.3g / L. Weigh the above chemical reagents with a balance, dissolve them in ultrapure water in a 1000ml beaker, stir the solution with a magnetic stirrer until it is clear, adjust the pH value of the solution to 4.5±0.1 with dilute sulfuric acid solution or sodium hydroxide solution, and use a heating device to control the initial temperature of the plating solution to 75±1℃.

[0058] (2) Use computer to control current density and additive concentration:

[0059] Current density: During the entire electrochemical deposition process, the current density remained constant at 30 mA / cm 2 .

[0060] At the same time, the concentration of the additive saccharin sodium was regulated: the concentration of saccharin sodium was maintained at 0.5 g / L within 1 hour after the start of electrochemical deposition, and then the concentration of saccharin sodium gradually increased from 0.5 g / L to 1.04 g / L within 1-1.5 hours, and then the concentration of saccharin sodium gradually increased from 1.04 g / L to 1.69 g / L within 1 hour, and then the concentration of saccharin sodium gradually increased from 1.69 g / L to 2.66 g / L within 1 hour, and then the concentration of saccharin sodium gradually increased from 2.66 g / L to 3.92 g / L within 1 hour, and then the concentration of saccharin sodium gradually increased from 3.92 g / L to 5.5 g / L within 1 hour, and finally the concentration of saccharin sodium remained unchanged at 5.5 g / L within the next 1.5 hours.

[0061] At the same time, the concentration of the additive cobalt sulfate heptahydrate was regulated: the concentration of cobalt sulfate heptahydrate was maintained at 0 g / L within 1 hour after the start of electrochemical deposition, and then the concentration of cobalt sulfate heptahydrate was gradually increased from 0 g / L to 5 g / L within 1 hour, and then the concentration of cobalt sulfate heptahydrate was gradually increased from 5 g / L to 80 g / L within the next 4 hours, and finally the concentration of cobalt sulfate heptahydrate was kept unchanged at 80 g / L within the next 1.5 hours.

[0062] Simultaneously, the temperature of the plating solution is controlled in the following manner:

[0063] Stage a: controlling the temperature of the plating solution to 75°C within 1-1.5 hours after the start of electrochemical deposition;

[0064] Stage b: within 0.5-1h after the end of stage a, the temperature of the plating solution is adjusted to 64-66°C;

[0065] Stage c: within 1-1.5 hours after the end of stage b, the temperature of the plating solution is adjusted to 59-61°C;

[0066] Stage d: maintaining the temperature of the plating solution at 59-61° C. within 4 hours after the end of stage c;

[0067] Stage e: Adjust the temperature to 44-46°C within 0.5-1h after the end of stage d;

[0068] The temperature adjustment in the stages b, c, e and f is all uniform.

[0069] The gradient structure nickel-cobalt alloy sample II was prepared in this embodiment. Figure 2 As shown in Figures ab, the grain size of sample II gradually refines from micrometer level to nanometer level, and there is no obvious macro interface. The coating quality is good without obvious micro cracks.

[0070] Phase distribution reference of electrochemically deposited gradient structure nickel-cobalt alloy sample II Figure 2 As shown in c, it can be seen that from the matrix to the surface, the phase structure gradually changes from single-phase FCC to dual-phase FCC+HCP structure.

[0071] Cross-sectional distribution of cobalt content and nickel content of electrochemically deposited gradient structure nickel-cobalt alloy sample II Figure 2 As shown in Figure d, it can be seen that the cobalt content gradually increases from 0 at% to ~82 at%.

[0072] Reference for the cross-sectional hardness distribution of gradient structure nickel-cobalt alloy Figure 2 As shown in Figure e, the hardness first increases rapidly from 2 GPa to 5.1 GPa, and then remains at around 5.1 GPa.

[0073] Example 3

[0074] This embodiment provides a method for preparing a gradient structure nickel-cobalt alloy, which comprises the following steps:

[0075] (1) In this embodiment, a metal nickel plate with a purity of 99.6% is used as a consumable anode, and a metal titanium plate is used as a cathode.

[0076] Prepare 1000ml of plating solution. The basic plating solution includes the following chemical reagents: NiSO4·6H2O: 100g / L, NaBr: 30g / L, H3BO3: 30g / L, C7H8NNaO5S: 0.5g / L, C 12 H 25SO4Na: 0.3g / L. Weigh the above chemical reagents with a balance, dissolve them in ultrapure water in a 1000ml beaker, stir the solution with a magnetic stirrer until it is clear, adjust the pH value of the solution to 4.5±0.1 with dilute sulfuric acid solution or sodium hydroxide solution, and use a heating device to control the initial temperature of the plating solution to 75±1℃.

[0077] (2) Use computer to control current density and additive concentration:

[0078] Current density: During the entire electrochemical deposition process, the current density remains constant at 30 mA / cm in 0-14 hours. 2 , increasing to 50 mA / cm within 14–19 hours 2 Finally, maintain 50mA / cm within 19-22h 2 .

[0079] At the same time, the concentration of the additive sodium saccharin was regulated: it was maintained at 0.5 g / L within 3 hours after the start of electrochemical deposition, the amount of sodium saccharin was increased to 5.5 g / L within the next 16 hours, and then the concentration was maintained unchanged within the last 3 hours until the end of deposition.

[0080] At the same time, the concentration of the additive cobalt sulfate heptahydrate was regulated: the concentration of cobalt sulfate heptahydrate was maintained at 0 g / L within 3 hours after the start of electrochemical deposition, and then the concentration of cobalt sulfate heptahydrate was gradually increased from 0 g / L to 6 g / L within 3 hours, and then the concentration of cobalt sulfate heptahydrate was gradually increased from 6 g / L to 18 g / L within 8 hours, and then the concentration of cobalt sulfate heptahydrate was increased to 120 g / L within 5 hours, and finally the concentration of cobalt sulfate heptahydrate was kept unchanged at 120 g / L within the next 3 hours.

[0081] Simultaneously, the temperature of the plating solution is controlled in the following manner:

[0082] Stage a: controlling the temperature of the plating solution to 75° C. within 3 hours after the start of electrochemical deposition;

[0083] Stage b: within 3 hours after the end of stage a, the temperature of the plating solution is adjusted to 64-66°C;

[0084] Stage c: within 8 hours after the end of stage b, the temperature of the plating solution is adjusted to 59-61°C;

[0085] Stage d: within 5 hours after the end of stage c, the temperature of the plating solution is adjusted to 49-51°C;

[0086] Stage e: within 3 hours after the end of stage d, the temperature of the plating solution is adjusted to 45-46°C;

[0087] The temperature adjustment in the stages b, c, e and f is all uniform.

[0088] The gradient structure nickel-cobalt alloy sample III was prepared in this embodiment. Figure 3 As shown in Figures ab, the grain size of sample III gradually refines from micron level to nanometer level, and there is no obvious macro interface. The coating quality is good without obvious micro cracks.

[0089] Phase distribution reference of electrochemically deposited gradient structure nickel-cobalt alloy sample III Figure 3 As shown in c, it can be seen that from the matrix to the surface, the phase structure is a single-phase FCC structure.

[0090] Cross-sectional distribution of cobalt content and nickel content of electrochemically deposited gradient structure nickel-cobalt alloy sample III Figure 3 As shown in Figure d, it can be seen that the cobalt content gradually increases from 0 at% to 75 at%, and then slowly decreases to 64 at%.

[0091] Reference for the cross-sectional hardness distribution of gradient structure nickel-cobalt alloy Figure 3 As shown in Fig. e, the hardness gradually increases from 2 GPa to 5.25 GPa, and then remains at around 5.25 GPa.

[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a nickel-cobalt alloy with a multi-gradient structure, characterized in that: The method comprises the following steps: adopting electrochemical deposition, taking nickel as a consumable anode, controlling the current density to increase gradually, controlling the cobalt salt concentration in the electroplating solution to increase gradually over time, controlling the concentration of sodium saccharin to increase gradually, and controlling the plating solution temperature, and depositing under the action of direct current to form a triple gradient structure nickel-cobalt alloy having a composite of grain size gradient, composition gradient and phase structure gradient.

2. The method according to claim 1, characterized in that The plating solution used for electrochemical deposition includes nickel sulfate hexahydrate with a concentration of 100±10g / L, sodium bromide with a concentration of 30±3g / L, boric acid with a concentration of 30±3g / L, and sodium dodecyl sulfate with a concentration of 0.3±0.03g / L; the pH of the plating solution is adjusted to 4.5±0.1; and the temperature of the plating solution is 45-75°C.

3. The method according to claim 2, characterized in that The cathode is titanium, copper, copper alloy, steel or nickel.

4. The method according to claim 3, characterized in that During the deposition process, the current density was from 30 mA / cm 2 Gradually increase to 50mA / cm 2 .

5. The method according to claim 4, characterized in that The cobalt salt is cobalt sulfate heptahydrate; during the deposition process, the concentration of cobalt sulfate heptahydrate is controlled to gradually increase from 0 g / L to 80 g / L.

6. The method according to claim 5, characterized in that The concentration of saccharin sodium is controlled to gradually increase from 0.5 g / L to 5.5 g / L; specifically, the concentration of saccharin sodium is maintained at 0.5 g / L within 1 hour after the start of electrochemical deposition, and then the concentration of saccharin sodium is gradually increased from 0.5 g / L to 1.04 g / L within 1-1.5 hours, and then the concentration of saccharin sodium is gradually increased from 1.04 g / L to 1.69 g / L within 1 hour, and then the concentration of saccharin sodium is gradually increased from 1.69 g / L to 2.66 g / L within 1 hour, and then the concentration of saccharin sodium is gradually increased from 2.66 g / L to 3.92 g / L within 1 hour, and then the concentration of saccharin sodium is gradually increased from 3.92 g / L to 5.5 g / L within 1 hour, and finally the concentration of saccharin sodium is maintained at 5.5 g / L within the next 1.5 hours.

7. The method according to claim 5, characterized in that During electrochemical deposition, the temperature of the plating solution is controlled as follows: Stage a: Control the temperature of the plating solution to 75°C within 1-1.5 hours after the start of electrochemical deposition; Stage b: within 0.5-1h after the end of stage a, adjust the temperature of the plating solution to 64-66°C; Stage c: Adjust the temperature of the plating solution to 59-61°C within 1-1.5 hours after the end of stage b; Stage d: Keep the temperature of the plating solution at 59-61°C within 4-5 hours after the end of stage c; Stage e: within 1-1.5 hours after the end of stage d, adjust the temperature of the plating solution to 49-51°C; Stage f: Adjust the temperature to 44-46°C within 0.5-1.5 hours after the end of stage e; The temperature in stages b, c, e and f is adjusted at a uniform speed.

8. The method according to claim 7, characterized in that The substrate is pretreated before deposition, specifically: mechanical polishing and surface degreasing of the substrate; Mechanical grinding and polishing specifically includes using 800#, 1000# and 1500# sandpaper to grind the surface of the substrate in sequence; Surface degreasing is the process of cleaning the substrate surface with an organic solvent.

9. A multi-gradient structure nickel-cobalt alloy, characterized in that: The method according to any one of claims 1 to 8 is used for preparation, wherein the grain size gradually transitions from micron-sized coarse crystals to nano-sized crystals along the deposition direction, the cobalt content gradually increases along the deposition direction, and the single-phase face-centered cubic structure gradually changes to a dual-phase structure in which face-centered cubic and close-packed hexagonal coexist.

10. The multi-gradient structure nickel-cobalt alloy according to claim 9, characterized in that: The grain size of gradient structure nickel-cobalt alloy is gradually refined from 10-20μm to 20-40nm; The atomic percentage of cobalt in the gradient structure nickel-cobalt alloy ranges from 0 to 82%.