Surface anti-corrosion treatment method for low-energy-consumption aluminum alloy part
By improving the thermoelectrochemical oxidation treatment of electrolyte and electrical parameters, the porosity problem in the surface oxidation process of aluminum alloy is solved, and a dense oxide layer with low energy consumption and high efficiency is achieved, meeting the anti-corrosion needs in the fields of aerospace and other fields.
Patent Information
- Application Number
- CN202411112366.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
AI Technical Summary
There are pore problems in the existing aluminum alloy surface oxidation process, which leads to insufficient corrosion resistance and mechanical strength of coatings, and the high energy consumption of micro-arc oxidation processes is not conducive to promotion.
By improving the electrolyte and electrical parameters, thermoelectrochemical oxidation treatment is used to form a dense oxide layer without additional sealing steps, reducing the current density, improving the density of the oxide layer and protecting effect.
It realizes a dense oxide layer without pores, reduces energy consumption, improves the corrosion protection performance of aluminum alloy parts, and meets the anti-corrosion needs in the fields of aerospace and other fields.
Smart Images

Figure CN119061450A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, in particular to a low-energy consumption aluminum alloy part surface anti-corrosion treatment method. Background Art
[0002] Aluminum alloy is an alloy with aluminum as the base material and a certain amount of other alloying elements added. It is one of the light metal materials and is widely used in aerospace, aviation, railway transportation, construction, electromechanical and other fields. The anti-corrosion performance of aluminum alloy is one of the key performances concerned in the above application fields. Under the conditions of most good service environments, aluminum alloy does not need additional anti-corrosion treatment. However, for some areas with particularly harsh service environments, such as areas around chemical enterprises, areas with corrosive substances such as salt, alkali and acid in the air, marine salt spray and dry-wet alternating environment, aerospace high-temperature thermal corrosion environment, etc., additional anti-corrosion treatment is required to meet the anti-corrosion performance requirements. Since aluminum alloy will form a natural oxide film in the air, the anti-corrosion technologies such as plasma spraying, paint coating, hot-dip galvanizing, etc. applicable to steel have problems such as weak bonding, easy detachment of coating, and short service life on aluminum alloy. Therefore, aluminum alloy parts are mainly formed through passivation, anodizing, micro-arc oxidation, thermo-electrochemical oxidation and other processes to form a dense oxide layer, thereby improving the anti-corrosion performance.
[0003] In various surface oxidation processes of aluminum alloys, since the workpiece to be treated is used as the anode, an electrochemical reaction in the electrolyte system is carried out under the action of an external power supply to form an oxide layer. During the reaction, the aluminum alloy surface will inevitably form holes in the oxide layer due to the release of gas, which will affect the corrosion resistance, mechanical strength and other properties of the coating. In order to solve the hole problem, hydrothermal sealing, nanoparticle sealing and other processes are often used as post-treatment processes or strengthening processes of micro-arc oxidation or other surface oxidation processes to fill the holes in the oxide layer. However, the sealing process increases the complexity of the entire process system. At the same time, the micro-arc oxidation, thermo-electrochemical oxidation and other processes developed in recent years require a large current density per unit area of the sample and a high unit energy consumption (electricity consumption), which is not conducive to the application and promotion of these technologies.
[0004] Invention patent application CN 112647105 A discloses a method for sealing the pores of aluminum alloy micro-arc oxidation ceramic film, which fills aluminum sol into the pores of aluminum and aluminum alloy micro-arc oxidation film and seals the pores through superheated water vapor treatment to improve the corrosion resistance and wear resistance of the micro-arc oxidation film. The current density used in the micro-arc oxidation process of this method is 6-10A / dm 2 The duty cycle is 30-40%, the time is 20-40 minutes, and the aluminum sol used is the aluminum sol formed by stirring pseudo-boehmite in a nitric acid solution. After vacuum suction and filling into the micro-arc oxidation film, a secondary heat treatment with high-temperature water vapor is performed. Summary of the invention
[0005] In view of the above problems existing in the prior art, the present invention provides a low-energy consumption aluminum alloy part surface anti-corrosion treatment method. The method of the present invention solves the pore problem of oxidation processes such as ordinary micro-arc oxidation by improving the coordination of electrolyte and electrical parameters. No additional sealing step is required, and the treatment has a good corrosion protection effect. The technical solution of the present invention is as follows:
[0006] The purpose of the present invention is to provide a low-energy consumption aluminum alloy part surface anti-corrosion treatment method, comprising the following steps:
[0007] (1) Check cast or forged aluminum alloy parts to ensure that there is no obvious damage, oil stains, or oxide scale on the surface;
[0008] (2) immersing the aluminum alloy parts in an electrolyte for thermal electrochemical oxidation treatment;
[0009] The electrolyte is prepared from oxalic acid, tartaric acid, malic acid and deionized water; the concentration of oxalic acid in the electrolyte is 10-50g / L, the concentration of tartaric acid is 10-20g / L, and the concentration of malic acid is 10-20g / L.
[0010] In one embodiment of the present invention, in step (1), the material of the aluminum alloy part is ZL101A, 2024 or 6082.
[0011] In one embodiment of the present invention, in step (2), during the thermoelectric oxidation treatment: the aluminum alloy part is connected to the anode of the pulse power supply, and the metal electrode is connected to the cathode of the pulse power supply.
[0012] In one embodiment of the present invention, in step (2), the thermoelectric oxidation treatment conditions are: the positive current of the pulse power supply is 2-4A / dm 2 , negative current is 2-4A / dm 2 , the duty cycle is 70-100%, and the reaction time is 120-150min.
[0013] In one embodiment of the present invention, after the thermo-electrochemical oxidation treatment, the surface oxide layer thickness of the aluminum alloy part is 40-60 μm, and the surface roughness Ra is 2.0-3.0 μm.
[0014] In one embodiment of the present invention, the protection level of the aluminum alloy parts after the thermal electrochemical oxidation treatment in the copper ion accelerated salt spray test for 96 hours is Rp8 or above.
[0015] In one embodiment of the present invention, after the thermal electrochemical oxidation treatment, SEM electron microscope observation combined with EDS energy spectrum element analysis of the aluminum alloy parts found that there were almost no pores in the oxide layer, and only a small amount of particles formed by agglomeration of silicon elements filled in the oxide layer.
[0016] The beneficial technical effects of the present invention are:
[0017] The present invention solves the pore problem of oxidation processes such as ordinary micro-arc oxidation by improving the coordination of electrolyte and electrical parameters. No additional sealing step is required. Electron microscope observation also verifies the effect of eliminating pores. At the same time, the average current density is lower, the energy-saving effect is better, and the treatment has a good corrosion protection effect (copper ion accelerated salt spray test 96h protection level 8 or above); it can meet the application of aluminum alloy parts in fields with anti-corrosion requirements such as railway transportation, aerospace, and construction electromechanical. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a photo of the double-ear sample of the cast aluminum alloy ZL101A sleeve after the treatment in Example 1 after 96 hours of CASS test.
[0019] Figure 2 This is a schematic diagram of the wire cutting position of the double-ear sample of the cast aluminum alloy ZL101A sleeve after treatment in Example 1.
[0020] Figure 3 This is a cross-sectional SEM photograph of the double-ear sample of the cast aluminum alloy ZL101A sleeve obtained after wire cutting sampling after treatment in Example 1.
[0021] Figure 4 This is a cross-sectional EDS energy spectrum element analysis photograph of the cast aluminum alloy ZL101A sleeve double-ear sample obtained after wire cutting sampling after the treatment in Example 1. DETAILED DESCRIPTION
[0022] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0023] The copper ion accelerated salt spray test and neutral salt spray test performed in the embodiments are carried out in accordance with GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test".
[0024] Embodiment 1:
[0025] A low-energy consumption aluminum alloy part surface anti-corrosion treatment method comprises the following steps:
[0026] (1) Check the cast aluminum alloy ZL101A sleeve double ear parts to ensure that there is no obvious damage, oil stains, or oxide scale on the surface;
[0027] (2) Oxalic acid, tartaric acid, malic acid and deionized water are mixed to prepare an electrolyte; the concentration of oxalic acid in the electrolyte is 30 g / L, the concentration of tartaric acid is 15 g / L, and the concentration of malic acid is 15 g / L.
[0028] (3) The cast aluminum alloy ZL101A sleeve double-ear part is connected to the anode of the pulse power supply, and the metal electrode is connected to the cathode of the pulse power supply. The cast aluminum alloy ZL101A sleeve double-ear part is immersed in the electrolyte prepared in step (2) for thermoelectrochemical oxidation treatment; the conditions of the thermoelectrochemical oxidation treatment are: the positive current of the pulse power supply is 4A / dm 2 , negative current is 4A / dm 2 , the duty cycle is 75% and the reaction time is 130 minutes.
[0029] After the treatment in this embodiment, the cast aluminum alloy ZL101A sleeve double-ear parts have a relatively smooth oxide layer with a thickness of 50 microns and a surface roughness Ra of 2.5 microns. The protection level of the copper ion accelerated salt spray test for 96 hours is Rp8 or above (such as Figure 1 ).
[0030] The center of the sleeve double-ear sample was selected for wire cutting, and the coating cross section on the outer surface was observed by SEM. Figure 2 As shown in Figure 2, SEM electron microscope observation combined with EDS energy spectrum element analysis found that there are almost no pores in the oxide layer, and only a small amount of silicon particles are formed by agglomeration and fill the oxide layer (such as Figure 3 , 4 ).
[0031] Embodiment 2:
[0032] A low-energy consumption aluminum alloy part surface anti-corrosion treatment method comprises the following steps:
[0033] (1) Check the cast aluminum alloy ZL101A sleeve double ear parts to ensure that there is no obvious damage, oil stains, or oxide scale on the surface;
[0034] (2) Oxalic acid, tartaric acid, malic acid and deionized water are mixed to prepare an electrolyte; the concentration of oxalic acid in the electrolyte is 50 g / L, the concentration of tartaric acid is 10 g / L, and the concentration of malic acid is 10 g / L.
[0035] (3) The cast aluminum alloy ZL101A sleeve double-ear part is connected to the anode of the pulse power supply, and the metal electrode is connected to the cathode of the pulse power supply. The cast aluminum alloy ZL101A sleeve double-ear part is immersed in the electrolyte prepared in step (2) for thermoelectrochemical oxidation treatment; the conditions of the thermoelectrochemical oxidation treatment are: the positive current of the pulse power supply is 3A / dm 2 , negative current is 3A / dm 2 , the duty cycle is 90% and the reaction time is 120 minutes.
[0036] After the treatment in this embodiment, the cast aluminum alloy ZL101A sleeve double-ear parts have a relatively smooth oxide layer with a thickness of 40 microns and a surface roughness Ra of 2.8 microns.
[0037] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A low-energy consumption aluminum alloy part surface anti-corrosion treatment method, characterized in that: The steps include: (1) Check cast or forged aluminum alloy parts to ensure that there is no obvious damage, oil stains, or oxide scale on the surface; (2) immersing the aluminum alloy parts in an electrolyte for thermal electrochemical oxidation treatment; The electrolyte is prepared from oxalic acid, tartaric acid, malic acid and deionized water; the concentration of oxalic acid in the electrolyte is 10-50g / L, the concentration of tartaric acid is 10-20g / L, and the concentration of malic acid is 10-20g / L.
2. The method for surface anticorrosion treatment of low-energy consumption aluminum alloy parts according to claim 1, characterized in that: In step (1), the material of the aluminum alloy part is ZL101A, 2024 or 6082.
3. The method for anticorrosion treatment of the surface of low-energy aluminum alloy parts according to claim 1, characterized in that: In step (2), during the thermoelectric oxidation treatment: the aluminum alloy part is connected to the anode of the pulse power supply, and the metal electrode is connected to the cathode of the pulse power supply.
4. The method for anticorrosion treatment of the surface of low-energy aluminum alloy parts according to claim 1, characterized in that: In step (2), the thermoelectric oxidation treatment conditions are: the positive current of the pulse power supply is 2-4A / dm 2 , negative current is 2-4A / dm 2 , the duty cycle is 70-100%, and the reaction time is 120-150min.
5. The method for anticorrosion treatment of the surface of low-energy aluminum alloy parts according to claim 1, characterized in that: After the thermo-electrochemical oxidation treatment, the surface oxide layer thickness of the aluminum alloy parts is 40-60 μm, and the surface roughness Ra is 2.0-3.0 μm.