Growth method and growth device of silicon carbide crystals

CN119061469AInactive Publication Date: 2024-12-03JIANGSU CHAOXINXING SEMICON CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411201900.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing silicon carbide crystal growth methods face challenges in maintaining stable vacuum pressure control, leading to safety hazards and limitations in achieving high temperatures and pressures, which affect the quality and size of the crystals.

Method used

A high-precision vacuum pressure control system is implemented, using a single-side opening quartz tube with a sealing member, crucible assembly, and a PID controller to stabilize pressure fluctuations, combined with a cooling system for improved temperature control and gas distribution.

Benefits of technology

This system enhances the safety and efficiency of crystal growth by reducing pressure fluctuations, allowing for higher temperatures and pressures, thereby improving the quality and size of silicon carbide crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061469A_ABST
    Figure CN119061469A_ABST
Patent Text Reader

Abstract

The invention provides a growth method and a growth device of silicon carbide crystals, and belongs to the field of silicon carbide crystal growth. The silicon carbide crystal growth device comprises a crystal growth furnace body, a quartz tube with an opening in one side is arranged in the crystal growth furnace body, and a sealing piece is installed at the opening end of the quartz tube in a sealed mode. A crucible assembly is arranged in the growth chamber of the quartz tube, the crucible assembly is provided with a first chamber and a second chamber, and the second chamber is located on the inner side of the first chamber; the crucible assembly is provided with an air inlet, an air inlet channel, an air outlet and an air outlet channel, the air inlet end of the air inlet channel is communicated with an air source, and an electric needle valve is arranged on a pipeline between the air source and the sealing element; an air outlet end of the air outlet channel is communicated with a vacuum pump; an electric ball valve is arranged on a pipeline between the vacuum pump and the sealing element; a pressure measuring hole is formed in the sealing piece and used for being externally connected with a vacuum gauge, and the vacuum gauge is connected with the input end of the PID controller and used for regulating and controlling the pressure of the growth cavity; and the crystal growth furnace body is externally connected with a vacuum system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of silicon carbide crystal growth, and in particular relates to a silicon carbide crystal growth method and a growth device. Background Art

[0002] As a new generation of industrially produced semiconductor materials, silicon carbide has excellent properties such as wide bandgap, high breakdown field strength, high thermal conductivity, high temperature stability and low dielectric constant. It is widely used in high power, high voltage, high frequency and other electronic device fields.

[0003] At present, the growth of silicon carbide single crystals generally adopts the physical vapor transport method (PVT). Since the ultimate goal of growing silicon carbide single crystals is to obtain large-sized, low-defect silicon carbide single crystals, as the size of silicon carbide single crystals increases, the vacuum pressure in the crystal growth furnace and the temperature control of the growth environment are extremely demanding. The change of process gas pressure and the setting of growth temperature have a great influence on the growth rate and crystal quality of silicon carbide crystals.

[0004] In order to stably control the temperature and pressure in the crystal growth furnace, the existing silicon carbide growth chamber is usually equipped with inlet and outlet holes at the upper and lower ends. Therefore, sealing structures need to be respectively provided at the upper and lower ends of the crystal growth furnace body. However, the two-layer sealing structure needs to be exposed to high-temperature radiation environment for a long time. The baked and aged sealing structure needs to be replaced in time to avoid major safety hazards such as sealing leakage.

[0005] Due to the limitations of crystal growth furnace and crystal growth process design, the current maximum crystal growth temperature achieved by PVT often does not exceed 2500℃. Accordingly, in order to ensure the quality of the crystal, the pressure in the furnace is required to be designed to a lower value. However, there is a certain fluctuation range in the gas pressure control, and this range accounts for a large proportion of the total pressure value.

[0006] Therefore, how to reduce safety hazards, lower the proportion of air pressure fluctuation range and accurately control air pressure are technical problems that need to be solved urgently. Summary of the invention

[0007] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a method and device for growing silicon carbide crystals. The present invention eliminates the influence of pressure fluctuations on the quality of crystal growth by setting a high-precision vacuum pressure control system, and improves the structure of the crystal growth furnace. By changing the quartz tube to a single-side opening and sealing only one end of the growth cavity, the safety hazards caused by the sealing work are reduced. At the same time, the use area of ​​the quartz tube is increased, and the cooling effect on the entire device is better, thereby effectively supporting the crystal growth work in a high-temperature environment, increasing the overall service life of the crystal growth furnace structure, and appropriately increasing the temperature and pressure in the crystal growth furnace, reducing the difficulty of low-pressure control in the crystal growth furnace, and obtaining silicon carbide crystals with better quality.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a silicon carbide crystal growth device, the silicon carbide crystal growth device comprises a crystal growth furnace body, a quartz tube with a single-side opening is arranged in the crystal growth furnace body, and a sealing member is sealed and installed at the open end of the quartz tube;

[0010] A crucible assembly is arranged in the growth chamber of the quartz tube, the crucible assembly has a first chamber and a second chamber, the second chamber is located inside the first chamber, a seed crystal is arranged on the top of the first chamber, and silicon carbide raw material is placed in the second chamber;

[0011] The crucible assembly has an air inlet, an air inlet channel, an air outlet and an air outlet channel, wherein the air inlet is located at the air outlet end of the air inlet channel and is connected to the second chamber; the air inlet channel runs through the bottom of the second chamber, and the air inlet end of the air inlet channel is connected to the gas source outside the crystal growth furnace body, and an electric needle valve is provided on the pipeline between the gas source and the sealing member;

[0012] The inlet channel and the inlet port are used to blow in a crystal growth auxiliary gas to drive the gas generated by the heating of the silicon carbide raw material in the second chamber to enter the first chamber from the second chamber and deposit on the seed crystal; the outlet port is located at the inlet end of the outlet channel, connected to the first chamber, and is used to discharge excess gas; the outlet end of the outlet channel is connected to a vacuum pump, and an electric ball valve is provided on the pipeline between the vacuum pump and the sealing member;

[0013] The sealing member is provided with a pressure measuring hole for connecting an external vacuum gauge, and the vacuum gauge is connected to the input end of the PID controller for regulating the pressure of the growth chamber;

[0014] The crystal growth furnace is externally connected to a vacuum system.

[0015] The present invention eliminates the influence of pressure fluctuations on crystal growth quality by arranging a high-precision vacuum pressure control system, and makes structural improvements to the crystal growth furnace. By changing the quartz tube to a single-side opening and sealing only one end of the growth chamber, the safety hazard caused by the sealing work is reduced. At the same time, the use area of ​​the quartz tube is increased, and the cooling effect on the entire device is better, thereby effectively supporting the crystal growth work in a high-temperature environment and increasing the overall service life of the crystal growth furnace structure. At the same time, the temperature and pressure in the crystal growth furnace are appropriately increased, the difficulty of low-pressure control in the crystal growth furnace is reduced, and silicon carbide crystals with better quality are obtained.

[0016] In the present invention, the second chamber is arranged on the inner side of the first chamber, and all directions and parts of the second chamber can stably and evenly receive the heat of the first chamber, so that the silicon carbide raw material in the second chamber is heated more evenly, the sublimation effect is good, and the generation of Si2C and SiC2 is reduced.

[0017] Preferably, the sealing assembly comprises a flange.

[0018] Preferably, the crucible assembly is coaxially arranged on the crucible supporting platform, and one end of the crucible supporting platform away from the crucible assembly is fixed on the sealing member.

[0019] Preferably, the crucible assembly comprises an outer crucible and an inner crucible.

[0020] Preferably, a crucible cover is sealed at the top open end of the outer crucible for fixing the seed crystal; a connecting shaft tube is provided on the radial inner side of the inner crucible, and the connecting shaft tube axially penetrates the inner crucible, the outer crucible and the seal.

[0021] Preferably, the outer wall of the inner crucible and the inner wall of the outer crucible define a first chamber, and the inner wall of the inner crucible and the outer wall of the connecting shaft tube define a second chamber.

[0022] Preferably, the inner wall of the connecting shaft tube defines an air inlet channel; and an air outlet channel is provided through the bottom of the outer crucible, the crucible support platform and the sealing member.

[0023] Preferably, the density of the inner crucible is ≤1.5 g / cm 3 , for example, it can be 1.5 g / cm 3 , 1.2g / cm 3 , 1g / cm 3 or 0.8g / cm 3 The porosity is ≥ 60%, for example, it can be 60%, 65%, 70% or 75%, etc.

[0024] Preferably, the inner crucible and the outer crucible are not in contact with each other, and the connecting shaft tube is rotationally connected to the inner crucible at a rotation rate of 0.1-10 rpm, for example, 0.1 rpm, 1 rpm, 3 rpm, 5 rpm, 7 rpm or 9 rpm.

[0025] In the present invention, the connecting shaft tube is rotatably connected to the crucible, so the second chamber rotates relative to the first chamber while discharging the silicon carbide gas, which can further promote the uniform distribution of the silicon carbide gas in the first chamber, thereby facilitating the uniform deposition of the gas on the surface of the seed crystal.

[0026] Preferably, the diameter of the air inlet is 6-10 mm, for example, 6 mm, 7 mm, 8 mm, 9 mm or 10 mm, and the diameter of the air outlet is 4-8 mm, for example, 4 mm, 5 mm, 6 mm, 7 mm or 8 mm.

[0027] In the present invention, the air inlet is used to blow crystal growth auxiliary gas into the crystal growth furnace, and at the same time can drive the gas generated by the raw material in the second chamber to enter the first chamber from the second chamber. If the diameter of the air inlet is too small, the gas cannot be evenly distributed in the crystal growth furnace; if the diameter of the air inlet is too large, the flow direction of the gas phase silicon carbide due to the temperature gradient will be greatly disturbed by the blown gas.

[0028] In the present invention, the gas outlet is used to discharge excess gas. If the diameter of the gas outlet is too small, the gas in the crystal growth furnace will not be discharged smoothly; if the diameter of the gas outlet is too large, it will affect the uniform distribution of gas in the crystal growth furnace and the heat field distribution in the crucible.

[0029] Preferably, the depth of the connecting shaft tube penetrating into the inner crucible is less than or equal to 3 / 4 of the axial height of the inner crucible.

[0030] Preferably, the opening diameter of the top opening of the inner crucible is 1 / 2-2 / 3 of the outer diameter of the inner crucible, for example, 1 / 2, 7 / 12 or 2 / 3.

[0031] Preferably, the vacuum gauge is a capacitance vacuum gauge.

[0032] Preferably, the measuring range of the vacuum gauge is 0.2-80 kPa, for example, it may be 0.2 kPa, 1 kPa, 10 kPa, 20 kPa, 30 kPa, 40 kPa, 50 kPa, 60 kPa, 70 kPa or 80 kPa, etc.

[0033] Preferably, the vacuum gauge comprises a first vacuum gauge and a second vacuum gauge, and the measuring range of the first vacuum gauge is smaller than the measuring range of the second vacuum gauge.

[0034] It should be noted that the first vacuum gauge may be a 10Torr vacuum gauge or a 1Torr vacuum gauge, and the second vacuum gauge may be a 1000Torr vacuum gauge.

[0035] Preferably, the first vacuum gauge is connected to a main input terminal of the PID controller, and the second vacuum gauge is connected to an auxiliary input terminal of the PID controller.

[0036] In the present invention, the PID controller will automatically switch to a vacuum gauge of a corresponding range according to the actual pressure in the crystal growth furnace, and the measurement signal of the vacuum gauge will be transmitted to the PID controller, which will drive the upstream electric needle valve and the downstream electric ball valve respectively, so that the closed-loop control circuit can realize precise control of the vacuum pressure within the full range. When the pressure control set value is in the high pressure range greater than 1 kPa, the PID controller is in the downstream control mode, the PID controller adjusts the upstream electric-controlled needle valve to a constant opening, and performs PID automatic adjustment on the downstream electric-controlled ball valve, and the pressure measurement value in the growth container is quickly equal to the set value by quickly adjusting the opening change of the electric-controlled ball valve; when the pressure control set value is in the low pressure range less than 1 kPa, the PID controller is in the upstream control mode, the PID controller adjusts the downstream electric-controlled ball valve to a constant opening, and performs PID automatic adjustment on the upstream electric-controlled needle valve, and the pressure measurement value in the growth container is quickly equal to the set value by quickly adjusting the opening change of the electric-controlled needle valve.

[0037] Preferably, the response time of the electric needle valve and the electric ball valve is less than 1 s, for example, it may be 0.8 s, 0.5 s or 0.3 s.

[0038] In the present invention, in order to always control the positive and negative pressures at the set values, the adjustment speed of the valve plays a key role. The electric-controlled needle valve and the electric-controlled ball valve with a response time of less than 1s can quickly recover the pressure fluctuations caused by temperature and other factors and stabilize it to the set pressure.

[0039] Preferably, a cooling tube is provided in the tube cavity of the quartz tube for realizing an axial temperature gradient.

[0040] In the present invention, the heat absorbed by the cooling water near the top of the crystal growth furnace (i.e., the end of the quartz tube without a flange) is greater than the heat absorbed by the cooling water at the bottom (the end with a flange), forming an axial temperature gradient. In addition, the upper limit of the temperature gradient change can be further expanded by adjusting the size of the cooling tube opening. By controlling the temperature and flow rate of the cooling water, the axial temperature gradient can be adjusted and controlled, thereby controlling the growth quality and growth rate of the crystal.

[0041] Preferably, a heat-insulating structure is provided on the outer surface of the crucible assembly.

[0042] Preferably, the thermal insulation structure is graphite felt.

[0043] Preferably, the silicon carbide crystal growth device further comprises a heating device, which is located at the periphery of the quartz tube and is used for heating the silicon carbide raw material in the second chamber so that the silicon carbide raw material is heated to generate gas.

[0044] Preferably, the heating device is a heating coil.

[0045] Preferably, the silicon carbide crystal growing device further comprises a temperature detection device for monitoring the temperature inside the crucible assembly.

[0046] Preferably, the temperature detection device comprises an infrared thermometer.

[0047] Preferably, the silicon carbide crystal growth device also includes a sleeve, which is sleeved on the outside of the thermal insulation structure, and one end of the sleeve is fixed on the seal, and the other end is attached to the top of the thermal insulation structure; a gas inlet is provided on the seal surrounded by the sleeve, and a gas outlet is provided on the seal not surrounded by the sleeve.

[0048] The present invention takes into account that the blown air flow may cause disturbance to the gas phase silicon carbide which rises due to the axial temperature gradient, and therefore a sleeve is provided to solve the above problem.

[0049] Preferably, a through hole is formed at one end of the sleeve that is in contact with the top of the thermal insulation structure, and the through hole is circumferentially arranged on the end surface of the sleeve.

[0050] In the present invention, through holes are circumferentially provided at the top end of the sleeve to facilitate gas flow guidance.

[0051] In a second aspect, the present invention provides a method for growing a silicon carbide crystal, wherein the method adopts the silicon carbide crystal growing device as described in the first aspect for growth, and the method comprises the following steps:

[0052] S1, the first stage: start the vacuum system, exhaust the crystal growth furnace after sealing detection, evacuate the furnace, and then introduce crystal growth auxiliary gas into the furnace to the first pressure, and gradually increase the temperature in the furnace to the first temperature;

[0053] S2, second stage: after the first stage is completed, the pressure in the furnace is reduced to a second pressure, and the temperature is raised to a second temperature to carry out the second stage of crystal growth;

[0054] S3. After the second stage is completed, finishing treatment is performed to obtain the silicon carbide crystal.

[0055] In the present invention, the temperature and efficiency of crystal growth are further improved by setting the temperature with different gradients.

[0056] Preferably, before starting the vacuum system, the crystal growth furnace body is first heated and the crystal growth furnace is cooled simultaneously. During the heating process, the crystal growth furnace is cooled simultaneously. The cooling water temperature in the cooling pipe is 20-30°C, for example, it can be 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, and the flow rate is 10-25mL / s, for example, it can be 10mL / s, 15mL / s, 20mL / s or 25mL / s, etc.

[0057] It should be noted that during the first and second stages, the crystal growth furnace is cooled simultaneously. Compared with the crystal growth furnace structure sealed on both sides by seals, the crystal growth furnace sealed on one side has a quartz tube structure at the top, and the corresponding cooling effect is better than that of the seal, with excellent cooling effect.

[0058] Preferably, the crystal growth auxiliary gas includes Ar and N2.

[0059] It should be noted that the process of introducing crystal growth auxiliary gas is always carried out during the entire growth process.

[0060] Preferably, the first pressure is 70-90 kPa, for example, 70 kPa, 75 kPa, 80 kPa, 85 kPa or 90 kPa, etc., and the first temperature is 1800-2200°C, for example, 1800°C, 1900°C, 2000°C, 2100°C or 2200°C, etc.

[0061] Preferably, the time for the temperature in the furnace to rise to the first temperature is 5-10 hours, for example, it can be 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.

[0062] Preferably, in the process of raising the temperature in the furnace to the first temperature, the temperature of the cooling water in the cooling pipe is 8-18°C, for example, it can be 8°C, 10°C, 12°C, 14°C, 16°C or 18°C, and the flow rate is 15-50mL / s, for example, it can be 15mL / s, 20mL / s, 25mL / s, 30mL / s, 35mL / s, 40mL / s, 45mL / s or 50mL / s, etc.

[0063] Preferably, the second pressure is 5-8 kPa, such as 5 kPa, 6 kPa, 7 kPa or 8 kPa, etc., and the second temperature is 2500-2800°C, such as 2500°C, 2600°C, 2700°C or 2800°C, etc.

[0064] Preferably, the second stage crystal growth time is 50-200 h, for example, 50 h, 100 h, 150 h or 200 h.

[0065] During the second stage, the cooling water temperature in the cooling pipe is 5-15°C, for example, it can be 5°C, 7°C, 9°C, 11°C, 13°C or 15°C, and the flow rate is 20-55mL / s, for example, it can be 20mL / s, 25mL / s, 30mL / s, 35mL / s, 40mL / s, 45mL / s, 50mL / s or 55mL / s.

[0066] In the present invention, by setting multiple gradients of cooling water temperature, it is possible to effectively ensure further improvement of crystal growth temperature and efficiency.

[0067] Preferably, the step of finishing treatment includes: firstly increasing the pressure at a constant temperature, and then decreasing the temperature and increasing the pressure to room temperature.

[0068] Preferably, the constant temperature and pressure increase time is 20-40 hours, for example, it can be 20 hours, 25 hours, 30 hours, 35 hours or 40 hours.

[0069] It should be noted that room temperature refers to 25±5°C, for example, it can be 20°C, 25°C or 30°C, and room pressure refers to one atmosphere.

[0070] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0071] Compared with the prior art, the present invention has the following beneficial effects:

[0072] The present invention eliminates the influence of pressure fluctuations on crystal growth quality by arranging a high-precision vacuum pressure control system, and makes structural improvements to the crystal growth furnace. By changing the quartz tube to a single-side opening and sealing only one end of the growth chamber, the safety hazard caused by the sealing work is reduced. At the same time, the use area of ​​the quartz tube is increased, and the cooling effect on the entire device is better, thereby effectively supporting the crystal growth work in a high-temperature environment and increasing the overall service life of the crystal growth furnace structure. At the same time, the temperature and pressure in the crystal growth furnace are appropriately increased, the difficulty of low-pressure control in the crystal growth furnace is reduced, and silicon carbide crystals with better quality are obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 This is a schematic diagram of the structure of the silicon carbide crystal growth device provided in Example 1 of the present invention.

[0074] Figure 2 This is a schematic diagram of the gas flow in the silicon carbide crystal growth device provided in Example 1 of the present invention.

[0075] Figure 3 This is a schematic diagram of the structure of a sleeve in a silicon carbide crystal growth device provided in Example 4 of the present invention.

[0076] Among them, 1-outer crucible; 11-crucible cover; 111-seed crystal; 12-crucible support platform; 13-inner crucible; 131-first chamber; 132-second chamber; 14-connecting shaft tube; 2-insulation structure; 21-sleeve; 3-quartz tube; 4-flange; 5-heating coil; 6-air inlet; 61-electric needle valve; 62-air source; 7-air outlet; 71-electric ball valve; 72-vacuum pump; 8-PID controller; 9-vacuum capacitance meter; 10-vacuum system. DETAILED DESCRIPTION

[0077] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0078] It should be noted that the room temperature below refers to 25°C.

[0079] Example 1

[0080] This embodiment provides a silicon carbide crystal growth device, and its structural schematic diagram is as follows Figure 1 As shown, the silicon carbide crystal growth device comprises a crystal growth furnace body, in which a quartz tube 3 with a single-side opening is arranged, and a flange 4 is sealed and installed at the open end of the quartz tube 3;

[0081] A crucible assembly is arranged in the growth chamber of the quartz tube 3, and the crucible assembly has a first chamber 131 and a second chamber 132, wherein the second chamber 132 is located inside the first chamber 131, a seed crystal 111 is arranged on the top of the first chamber 131, and silicon carbide raw materials are placed in the second chamber 132;

[0082] The crucible assembly is coaxially arranged on the crucible support platform 12, and one end of the crucible support platform 12 away from the crucible assembly is fixed on the flange 4;

[0083] A heat-insulating structure 2 is provided on the outer surface of the crucible assembly, and the heat-insulating structure 2 is graphite felt;

[0084] The crucible assembly comprises an outer crucible 1 and an inner crucible 13, wherein the top open end of the outer crucible 1 is sealed with a crucible cover 11 for fixing a seed crystal 111; a connecting shaft tube 14 is arranged on the radial inner side of the inner crucible 13, and the connecting shaft tube 14 axially penetrates the inner crucible 13, the outer crucible 1 and the flange 4; the inner crucible 13 and the outer crucible 1 do not contact each other, and the connecting shaft tube 14 is rotationally connected to the inner crucible 13 at a rotation rate of 5 rpm; the outer wall of the inner crucible 13 and the inner wall of the outer crucible 1 define a first chamber 131, and the inner wall of the inner crucible 13 and the outer wall of the connecting shaft tube 14 define a second chamber 132;

[0085] The crucible assembly has an air inlet 6, an air inlet channel, an air outlet 7 and an air outlet channel, and the inner wall of the connecting shaft tube 14 defines the air inlet channel; the air outlet channel is provided through the bottom of the outer crucible 1, the crucible support platform 12 and the flange 4; the air inlet 6 is located at the air outlet end of the air inlet channel and is connected to the second chamber 132; the air inlet channel passes through the bottom of the second chamber 132, and the air inlet end of the air inlet channel is connected to the gas source 62 outside the crystal growth furnace body, and an electric needle valve 61 is provided on the pipeline between the gas source 62 and the flange 4;

[0086] Figure 2 The flow principle diagram of the gas in the silicon carbide crystal growth device provided in the present embodiment is shown. It can be seen from the figure that the air inlet channel and the air inlet 6 are used to blow the combination gas of N2 and Ar into the crystal growth furnace, and at the same time, the gas generated by the heating of the silicon carbide raw material in the second chamber 132 can be driven to enter the first chamber 131 from the second chamber 132 and deposit on the seed crystal 111. The air outlet 7 is located at the air inlet end of the air outlet channel, connected to the first chamber 131, and is used to discharge excess gas. The air outlet end of the air outlet channel is connected to the vacuum pump 72, and an electric ball valve 71 is provided on the pipeline between the vacuum pump 72 and the flange 4; the response time of the electric needle valve 61 and the electric ball valve 71 is less than 1s;

[0087] The diameter of the air inlet 6 is 10 mm, and the diameter of the air outlet 7 is 8 mm;

[0088] The flange 4 is provided with a pressure measuring hole for externally connecting a vacuum capacitance gauge 9, wherein the vacuum capacitance gauge 9 comprises a first capacitance vacuum gauge and a second capacitance vacuum gauge, wherein the first capacitance vacuum gauge is a 10Torr capacitance vacuum gauge, and the second capacitance vacuum gauge is a 1000Torr capacitance vacuum gauge, and the first capacitance vacuum gauge and the second capacitance vacuum gauge are respectively connected to a main input terminal and an auxiliary input terminal of a PID controller 8 for regulating the pressure of the growth chamber;

[0089] The crystal growth furnace is externally connected to a vacuum system 10;

[0090] The porosity of the inner crucible is 75%;

[0091] A cooling tube is provided in the tube cavity of the quartz tube 3 to achieve an axial temperature gradient;

[0092] The silicon carbide crystal growth device further includes a heating coil 5, which is located at the outer periphery of the quartz tube 3 and is used to heat the silicon carbide raw material in the second chamber 132 so that the silicon carbide raw material is heated to generate gas;

[0093] The silicon carbide crystal growth device also includes an infrared thermometer for monitoring the temperature inside the crucible assembly.

[0094] This embodiment also provides a method for growing a silicon carbide crystal based on the above-mentioned growth device, and the growth method comprises the following steps:

[0095] (1) In the first stage, the crystal growth furnace body is heated and cooled simultaneously. At this time, the cooling water temperature in the cooling pipe is 20°C and the flow rate is 25 mL / s. The vacuum system is started to perform a sealing test and then exhaust the air, and the pressure in the furnace is controlled to the process requirement value. The furnace is evacuated, and then a combination of N2 and Ar is introduced into the furnace to a first pressure, and the temperature in the furnace is raised to a first temperature.

[0096] The first pressure is 90 kPa, the first temperature is 2200° C., and the time for the temperature in the furnace to rise to the first temperature is 5 hours; during the process of raising the temperature in the furnace to the first temperature, the temperature of the cooling water in the cooling pipe is 8° C., and the flow rate is 50 mL / s;

[0097] (2) Second stage: After the first stage, the pressure in the furnace is reduced to a second pressure, and the temperature is increased to a second temperature to carry out the second stage of crystal growth;

[0098] The second pressure is 8 kPa, the second temperature is 2800° C., and the second stage crystal growth time is 150 h. During the second stage, the cooling water temperature in the cooling pipe is 5° C. and the flow rate is 55 mL / s.

[0099] (3) After the second stage of crystal growth is completed, the pressure is slowly increased to 10 kPa within 30 hours while keeping the temperature constant, and then the pressure is quickly increased to one atmosphere. After the temperature in the crystal growth furnace drops to room temperature, the crystal growth furnace is opened and the silicon carbide crystal grown in the crucible assembly is taken out.

[0100] Example 2

[0101] This embodiment provides a silicon carbide crystal growth device, which includes a crystal growth furnace body, in which a quartz tube with a single-side opening is arranged, and a flange is sealed and installed at the open end of the quartz tube;

[0102] A crucible assembly is arranged in the growth chamber of the quartz tube, the crucible assembly has a first chamber and a second chamber, the second chamber is located inside the first chamber, a seed crystal is arranged on the top of the first chamber, and silicon carbide raw material is placed in the second chamber;

[0103] The crucible assembly is coaxially arranged on the crucible support platform, and one end of the crucible support platform away from the crucible assembly is fixed on the flange;

[0104] A heat-insulating structure is provided on the outer surface of the crucible assembly, and the heat-insulating structure is graphite felt;

[0105] The crucible assembly comprises an outer crucible and an inner crucible, wherein the top open end of the outer crucible is sealed with a crucible cover for fixing a seed crystal; a connecting shaft tube is arranged on the radial inner side of the inner crucible, and the connecting shaft tube axially penetrates the inner crucible, the outer crucible and the flange; the inner crucible and the outer crucible are not in contact with each other, and the connecting shaft tube is rotationally connected to the inner crucible at a rotation rate of 1 rpm; the outer wall of the inner crucible and the inner wall of the outer crucible define a first chamber, and the inner wall of the inner crucible and the outer wall of the connecting shaft tube define a second chamber;

[0106] The crucible assembly has an air inlet, an air inlet channel, an air outlet and an air outlet channel, the inner wall of the connecting shaft tube defines the air inlet channel; the bottom of the outer crucible, the crucible support platform and the flange are provided with the air outlet channel; the air inlet is located at the air outlet end of the air inlet channel and is connected to the second chamber; the air inlet channel passes through the bottom of the second chamber, and the air inlet end of the air inlet channel is connected to the gas source outside the crystal growth furnace body, and an electric needle valve is provided on the pipeline between the gas source and the flange;

[0107] The inlet channel and the inlet port are used to blow a combination of N2 and Ar into the crystal growth furnace, and can also drive the gas generated by the heating of the silicon carbide raw material in the second chamber to enter the first chamber from the second chamber and deposit on the seed crystal. The outlet port is located at the inlet end of the outlet channel, connected to the first chamber, and is used to discharge excess gas. The outlet end of the outlet channel is connected to a vacuum pump, and an electric ball valve is provided on the pipeline between the vacuum pump and the flange. The response time of the electric needle valve and the electric ball valve is less than 1s.

[0108] The diameter of the air inlet is 8 mm, and the diameter of the air outlet is 6 mm;

[0109] The flange is provided with a pressure measuring hole for externally connecting a first capacitance vacuum gauge and a second capacitance vacuum gauge, wherein the first capacitance vacuum gauge is a 10Torr capacitance vacuum gauge, and the second capacitance vacuum gauge is a 1000Torr capacitance vacuum gauge, and the first capacitance vacuum gauge and the second capacitance vacuum gauge are respectively connected to a main input terminal and an auxiliary input terminal of a PID controller for regulating the pressure of the growth chamber;

[0110] The crystal growth furnace is externally connected to a vacuum system;

[0111] The porosity of the inner crucible is 75%;

[0112] A cooling tube is provided in the tube cavity of the quartz tube to achieve an axial temperature gradient;

[0113] The silicon carbide crystal growth device further includes a heating coil, which is located at the outer periphery of the quartz tube and is used to heat the silicon carbide raw material in the second chamber so that the silicon carbide raw material is heated to generate gas;

[0114] The silicon carbide crystal growth device also includes an infrared thermometer for monitoring the temperature inside the crucible assembly.

[0115] This embodiment also provides a method for growing a silicon carbide crystal based on the above-mentioned growth device, and the growth method comprises the following steps:

[0116] (1) The first stage: the crystal growth furnace body is heated and cooled simultaneously. At this time, the cooling water temperature in the cooling pipe is 25°C and the flow rate is 20 mL / s. After the vacuum system is started for sealing detection, the vacuum system is started for exhaust, the air is exhausted, and the pressure in the furnace is controlled to the process requirement value, and then a combination of N2 and Ar is introduced into the furnace to the first pressure, and the temperature in the furnace is raised to the first temperature;

[0117] The first pressure is 80 kPa, the first temperature is 2000° C., and the time for the temperature in the furnace to rise to the first temperature is 7 hours; during the process of raising the temperature in the furnace to the first temperature, the temperature of the cooling water in the cooling pipe is 12° C., and the flow rate is 30 mL / s;

[0118] (2) Second stage: After the first stage, the pressure in the furnace is reduced to a second pressure, and the temperature is increased to a second temperature to carry out the second stage of crystal growth;

[0119] The second pressure is 6 kPa, the second temperature is 2650° C., and the second stage crystal growth time is 180 h. During the second stage crystal growth, the cooling water temperature in the cooling tube is 10° C. and the flow rate is 40 mL / s.

[0120] (3) After the second stage of crystal growth is completed, the pressure is slowly increased to 10 kPa within 20 hours while keeping the temperature constant, and then the pressure is quickly increased to one atmosphere. After the temperature in the crystal growth furnace drops to room temperature, the crystal growth furnace is opened and the silicon carbide crystal grown in the crucible assembly is taken out.

[0121] Example 3

[0122] This embodiment provides a silicon carbide crystal growth device, which includes a crystal growth furnace body, in which a quartz tube with a single-side opening is arranged, and a flange is sealed and installed at the open end of the quartz tube;

[0123] A crucible assembly is arranged in the growth chamber of the quartz tube, the crucible assembly has a first chamber and a second chamber, the second chamber is located inside the first chamber, a seed crystal is arranged on the top of the first chamber, and silicon carbide raw material is placed in the second chamber;

[0124] The crucible assembly is coaxially arranged on the crucible support platform, and one end of the crucible support platform away from the crucible assembly is fixed on the flange;

[0125] A heat-insulating structure is provided on the outer surface of the crucible assembly, and the heat-insulating structure is graphite felt;

[0126] The crucible assembly comprises an outer crucible and an inner crucible, wherein the top open end of the outer crucible is sealed with a crucible cover for fixing a seed crystal; a connecting shaft tube is arranged on the radial inner side of the inner crucible, and the connecting shaft tube axially penetrates the inner crucible, the outer crucible and the flange; the inner crucible and the outer crucible are not in contact with each other, and the connecting shaft tube is rotationally connected to the inner crucible at a rotation rate of 10 rpm; the outer wall of the inner crucible and the inner wall of the outer crucible define a first chamber, and the inner wall of the inner crucible and the outer wall of the connecting shaft tube define a second chamber;

[0127] The crucible assembly has an air inlet, an air inlet channel, an air outlet and an air outlet channel, the inner wall of the connecting shaft tube defines the air inlet channel; the bottom of the outer crucible, the crucible support platform and the flange are provided with the air outlet channel; the air inlet is located at the air outlet end of the air inlet channel and is connected to the second chamber; the air inlet channel passes through the bottom of the second chamber, and the air inlet end of the air inlet channel is connected to the gas source outside the crystal growth furnace body, and an electric needle valve is provided on the pipeline between the gas source and the flange;

[0128] The inlet channel and the inlet port are used to blow a combination of N2 and Ar into the crystal growth furnace, and can also drive the gas generated by the heating of the silicon carbide raw material in the second chamber to enter the first chamber from the second chamber and deposit on the seed crystal. The outlet port is located at the inlet end of the outlet channel, connected to the first chamber, and is used to discharge excess gas. The outlet end of the outlet channel is connected to a vacuum pump, and an electric ball valve is provided on the pipeline between the vacuum pump and the flange. The response time of the electric needle valve and the electric ball valve is less than 1s.

[0129] The diameter of the air inlet is 6 mm, and the diameter of the air outlet is 4 mm;

[0130] The flange is provided with a pressure measuring hole for externally connecting a first capacitance vacuum gauge and a second capacitance vacuum gauge, wherein the first capacitance vacuum gauge is a 1Torr capacitance vacuum gauge, and the second capacitance vacuum gauge is a 1000Torr capacitance vacuum gauge, and the first capacitance vacuum gauge and the second capacitance vacuum gauge are respectively connected to a main input terminal and an auxiliary input terminal of a PID controller for regulating the pressure of the growth chamber;

[0131] The crystal growth furnace is externally connected to a vacuum system;

[0132] The porosity of the inner crucible is 75%;

[0133] A cooling tube is provided in the tube cavity of the quartz tube to achieve an axial temperature gradient;

[0134] The silicon carbide crystal growth device further includes a heating coil, which is located at the outer periphery of the quartz tube and is used to heat the silicon carbide raw material in the second chamber so that the silicon carbide raw material is heated to generate gas;

[0135] The silicon carbide crystal growth device also includes an infrared thermometer for monitoring the temperature inside the crucible assembly.

[0136] This embodiment also provides a method for growing a silicon carbide crystal based on the above-mentioned growth device, and the growth method comprises the following steps:

[0137] (1) The first stage: the crystal growth furnace body is heated and cooled simultaneously. At this time, the cooling water temperature in the cooling pipe is 30°C and the flow rate is 10 mL / s. After the vacuum system is started for sealing detection, the vacuum system is started for exhaust, the air is exhausted, and the pressure in the furnace is controlled to the process requirement value, and then a combination of N2 and Ar is introduced into the furnace to the first pressure, and the temperature in the furnace is raised to the first temperature;

[0138] The first pressure is 70 kPa, the first temperature is 1800° C., and the time for the temperature in the furnace to rise to the first temperature is 10 hours; during the process of raising the temperature in the furnace to the first temperature, the temperature of the cooling water in the cooling pipe is 18° C., and the flow rate is 15 mL / s;

[0139] (2) Second stage: After the first stage, the pressure in the furnace is reduced to a second pressure, and the temperature is increased to a second temperature to carry out the second stage of crystal growth;

[0140] The second pressure is 5 kPa, the second temperature is 2500° C., and the second stage crystal growth time is 200 h. During the second stage crystal growth process, the cooling water temperature in the cooling tube is 15° C. and the flow rate is 20 mL / s.

[0141] (3) After the second stage of crystal growth is completed, the pressure is slowly increased to 10 kPa within 40 hours while keeping the temperature constant, and then the pressure is quickly increased to one atmosphere. After the temperature in the crystal growth furnace drops to room temperature, the crystal growth furnace is opened and the silicon carbide crystal grown in the crucible assembly is taken out.

[0142] Example 4

[0143] The difference between this embodiment and embodiment 1 is that the silicon carbide crystal growth device provided in this embodiment further includes a sleeve, such as Figure 3 As shown, the sleeve 21 is sleeved on the outside of the thermal insulation structure, and one end of the sleeve 21 is fixed on the flange, and the other end is attached to the top of the graphite felt;

[0144] The flange surrounded by the sleeve 21 is provided with a gas inlet, and the flange not surrounded by the sleeve 21 is provided with a gas outlet;

[0145] A through hole is formed at one end of the sleeve 21 which is in contact with the top of the graphite felt. The through hole is circumferentially arranged on the end surface of the sleeve 21 .

[0146] The remaining structures, methods and parameters remain the same as those in Example 1.

[0147] Example 5

[0148] The difference between this embodiment and embodiment 1 is that the first capacitance vacuum gauge is not provided.

[0149] The remaining structures, methods and parameters remain the same as those in Example 1.

[0150] Comparative Example 1

[0151] The difference between this comparative example and Example 1 is that two opposite sides of the quartz tube are open, and flanges are sealed and installed at the open ends of the quartz tube.

[0152] The remaining structures, methods and parameters refer to the conventional PVT process, and the crystal growth temperature does not exceed 2500°C.

[0153] Comparative Example 2

[0154] The difference between this comparative example and Example 1 is that a PID controller and a vacuum gauge are not provided.

[0155] The remaining structures, methods and parameters remain the same as those in Example 1.

[0156] Comparative Example 3

[0157] The difference between this comparative example and Example 1 is that the second temperature in step (2) is the same as the first temperature in step (1).

[0158] The remaining structures, methods and parameters remain the same as those in Example 1.

[0159] Performance Testing

[0160] The silicon carbide crystals prepared in the above-mentioned embodiments and comparative examples were inspected using an optical defect inspection device.

[0161] The test results are shown in Table 1.

[0162] Table 1

[0163]

[0164] analyze:

[0165] In summary, the present invention eliminates the influence of pressure fluctuations on crystal growth quality by setting up a high-precision vacuum pressure control system, and makes structural improvements to the crystal growth furnace. By changing the quartz tube to a single-sided opening and only sealing one end of the growth chamber, the safety hazard caused by the sealing work is reduced. At the same time, the use area of ​​the quartz tube is increased, and the cooling effect on the entire device is better, thereby effectively supporting the crystal growth work in a high-temperature environment and increasing the overall service life of the crystal growth furnace structure. At the same time, the temperature and pressure in the crystal growth furnace are appropriately increased, which reduces the difficulty of low-pressure control in the crystal growth furnace and obtains silicon carbide crystals with better quality.

[0166] By comparing Example 1 with Example 4, it can be seen that adding a sleeve can help reduce the interference of the growth-assisting gas on the silicon carbide vapor phase growth process. At the same time, the design of providing the inlet and outlet ports inside and outside the sleeve can ensure that the growth-assisting gas is evenly distributed in the crystal growth furnace. After the thermal field adjustment design, it is similar to Example 1.

[0167] By comparing Example 1 with Example 5, it can be seen that if only one capacitance vacuum gauge is provided, only a single large-range vacuum gauge can be used, which makes it difficult to perform pressure accuracy control in the low-pressure range.

[0168] By comparing Example 1 with Comparative Example 1, it can be seen that if the two opposite sides of the quartz tube are open and the open ends of the quartz tube are sealed with flanges, the overall cooling effect of the crystal growth furnace is reduced, resulting in a corresponding decrease in the maximum crystal growth temperature and a decrease in the axial temperature gradient. At this time, the comparative example is consistent with the conventional crystal growth method, and the crystal quality is not significantly improved.

[0169] By comparing Example 1 with Comparative Example 2, it can be seen that if the PID controller and the vacuum gauge are not provided, the ratio of the pressure fluctuation to the total pressure will increase accordingly, and the pressure fluctuation difference of the part that cannot be accurately controlled will slightly cause a change in the crystal quality.

[0170] By comparing Example 1 with Comparative Example 3, it can be seen that if the temperature gradient of crystal growth is not set, the temperature during the actual crystal growth stage will be insufficient, which will lead to more problems in crystal quality, such as more inclusions, microtubes and total dislocations.

[0171] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A silicon carbide crystal growth device, characterized in that: The silicon carbide crystal growth device comprises a crystal growth furnace body, wherein a quartz tube with a single-side opening is arranged in the crystal growth furnace body, and a sealing member is installed at the open end of the quartz tube; A crucible assembly is arranged in the growth chamber of the quartz tube, the crucible assembly has a first chamber and a second chamber, the second chamber is located inside the first chamber, a seed crystal is arranged on the top of the first chamber, and silicon carbide raw material is placed in the second chamber; The crucible assembly has an air inlet, an air inlet channel, an air outlet and an air outlet channel, wherein the air inlet is located at the air outlet end of the air inlet channel and is connected to the second chamber; the air inlet channel runs through the bottom of the second chamber, and the air inlet end of the air inlet channel is connected to the gas source outside the crystal growth furnace body, and an electric needle valve is provided on the pipeline between the gas source and the sealing member; The inlet channel and the inlet port are used to blow in a crystal growth auxiliary gas to drive the gas generated by the heating of the silicon carbide raw material in the second chamber to enter the first chamber from the second chamber and deposit on the seed crystal; the outlet port is located at the inlet end of the outlet channel, connected to the first chamber, and is used to discharge excess gas; the outlet end of the outlet channel is connected to a vacuum pump, and an electric ball valve is provided on the pipeline between the vacuum pump and the sealing member; The sealing member is provided with a pressure measuring hole for connecting an external vacuum gauge, and the vacuum gauge is connected to the input end of the PID controller for regulating the pressure of the growth chamber; The crystal growth furnace is externally connected to a vacuum system.

2. The silicon carbide crystal growth device according to claim 1, characterized in that: The sealing assembly includes a flange; The crucible assembly is coaxially arranged on the crucible supporting platform, and one end of the crucible supporting platform away from the crucible assembly is fixed on the sealing member.

3. The silicon carbide crystal growth device according to claim 2, characterized in that: The crucible assembly includes an outer crucible and an inner crucible; The top open end of the outer crucible is sealed with a crucible cover for fixing the seed crystal; the radial inner side of the inner crucible is provided with a connecting shaft tube, and the connecting shaft tube axially penetrates the inner crucible, the outer crucible and the sealing member; The outer wall of the inner crucible and the inner wall of the outer crucible define a first chamber, and the inner wall of the inner crucible and the outer wall of the connecting shaft tube define a second chamber; The inner wall of the connecting shaft tube defines an air inlet channel; the bottom of the outer crucible, the crucible support platform and the sealing member are penetrated by an air outlet channel.

4. The silicon carbide crystal growth device according to claim 1, characterized in that: The vacuum gauge is a capacitance vacuum gauge; The measuring range of the vacuum gauge is 0.1Pa-100kPa; The vacuum gauge comprises a first vacuum gauge and a second vacuum gauge, wherein the measuring range of the first vacuum gauge is smaller than the measuring range of the second vacuum gauge; The first vacuum gauge is connected to the main input terminal of the PID controller, and the second vacuum gauge is connected to the auxiliary input terminal of the PID controller; The response time of the electric needle valve and the electric ball valve is less than 1s.

5. The silicon carbide crystal growth device according to claim 1, characterized in that: A cooling tube is provided in the tube cavity of the quartz tube to achieve an axial temperature gradient; A heat preservation structure is arranged on the outer surface of the crucible assembly; The silicon carbide crystal growth device further comprises a heating device, which is located at the periphery of the quartz tube and is used to heat the silicon carbide raw material in the second chamber so that the silicon carbide raw material is heated to generate gas; The silicon carbide crystal growing device also includes a temperature detection device for monitoring the temperature inside the crucible assembly.

6. The silicon carbide crystal growth device according to claim 5, characterized in that: The silicon carbide crystal growth device further comprises a sleeve, which is sleeved on the outside of the heat preservation structure, and one end of the sleeve is fixed on the sealing member, and the other end is attached to the top of the heat preservation structure; The sealing part surrounded by the sleeve is provided with a gas inlet, and the sealing part not surrounded by the sleeve is provided with a gas outlet; a through hole is opened at one end of the sleeve that is in contact with the top of the thermal insulation structure, and the through hole is circumferentially arranged on the end surface of the sleeve.

7. A method for growing silicon carbide crystals, characterized in that: The growth method adopts the silicon carbide crystal growth device according to any one of claims 1 to 6 for growth, and the growth method comprises the following steps: S1, the first stage: start the vacuum system, exhaust the crystal growth furnace after sealing detection, evacuate the furnace, and then introduce crystal growth auxiliary gas into the furnace to the first pressure, and gradually increase the temperature in the furnace to the first temperature; S2, second stage: after the first stage is completed, the pressure in the furnace is reduced to a second pressure, and the temperature is raised to a second temperature to carry out the second stage of crystal growth; S3. After the second stage is completed, finishing treatment is performed to obtain the silicon carbide crystal.

8. The growth method according to claim 7, characterized in that: The crystal growth assisting gas includes Ar and N2.

9. The growth method according to claim 7, characterized in that: The first pressure is 70-90 kPa, and the first temperature is 1800-2200° C.; The time for the temperature in the furnace to rise to the first temperature is 5-10 hours; When the temperature in the furnace is raised to the first temperature, the temperature of the cooling water in the cooling pipe is 8-18° C. and the flow rate is 15-50 mL / s.

10. The growth method according to claim 7, characterized in that: The second pressure is 5-8 kPa, and the second temperature is 2500-2800° C.; The second stage crystal growth time is 50-200h; During the second stage, the cooling water temperature in the cooling pipe is 5-15°C and the flow rate is 20-55mL / s; The steps of the finishing treatment include: firstly increasing the pressure at a constant temperature, and then decreasing the temperature and increasing the pressure to room temperature.

Citation Information

Patent Citations

  • Silicon carbide crystal growing device

    CN114108096A

  • Apparatus for growing silicon carbide single crystal

    KR101724290B1

  • Method for growing crystals

    US20230357951A1

  • Silicon carbide with low nitrogen content and method for preparation

    US8858709B1