Organic fiber, prepreg, metal-clad laminate, printed wiring board, and electronic device

Through the organic fibers with optimized characteristics, the problem of insufficient signal offset and dimensional stability in high-speed transmission is solved, and the dielectric performance and dimensional stability is improved, which is suitable for high-performance printed circuit boards.

CN119061525APending Publication Date: 2024-12-03ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410686202.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In high-speed transmission above 200 Gbps, the problem of signal shift (SKEW) is gradually becoming apparent, and the existing organic fibers have insufficient dimensional stability when they are substrates, prepregs and laminates.

Method used

Organic fibers containing more than 5% and less than 100% of the homostatic polystyrene are used, and the crystallographic size of 2θ=6.8° (110 surfaces) is 3 to 10 nm, the crystallization orientation degree is 0.92 or more, and the diameter of the monofilament is 1. ~50 μm, and contains more than 60% of the syndiotactic polystyrene and more than 5% of the amorphous polymer, for the preparation of prepregs and metal-covered laminates.

Benefits of technology

It achieves excellent dielectric constant, dielectric loss tangent and dimensional stability, reduces signal offset, improves spinning and thermal stress rise temperature, and is suitable for high-performance printed circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061525A_ABST
    Figure CN119061525A_ABST
Patent Text Reader

Abstract

Provided are an organic fiber, a prepreg, a metal-clad laminate, a printed wiring board, and an electronic device suitable for a fiber cloth that is a raw material for a laminate that satisfies excellent dielectric constant, dielectric loss tangent, and dimensional stability (low warpage). An organic fiber which contains 5-100 mass% of syndiotactic polystyrene, and which has a crystallite size at 2 [theta] = 6.8 DEG (110 plane) of 3-10 nm, a crystal orientation degree of 0.92 or more, and a monofilament diameter of 1-50 [mu] m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to organic fibers, prepregs, metal-clad laminates, printed circuit boards and electronic devices. Background Art

[0002] In recent years, along with the remarkable progress of information network technology or the expansion of the service of making use of information network, electronic equipment is required to have large capacity of information amount and high speed of processing speed.In order to meet these requirements, for the printed circuit board carried in electronic equipment, on the basis of the characteristics such as insulation reliability, rigidity, flame retardancy required in the past, low dielectric constant and low dielectric loss tangent are also strongly required.Therefore, for the main insulating material constituting printed circuit board, i.e. resin combination (hereinafter also the composition is referred to as matrix resin composition or thermosetting matrix resin composition) and the fiber cloth becoming its base material, the further improvement of dielectric constant and dielectric loss tangent has been studied.

[0003] As the matrix resin composition, a mixture of polyphenylene ether (hereinafter also referred to as PPE) having low dielectric constant and dielectric loss tangent and high heat resistance can be suitably used as the above-mentioned printed wiring board material.

[0004] For example, Patent Documents 1 and 2 disclose organic fibers containing PPE as a matrix resin composition.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application No. 2017-502179

[0008] Patent Document 2: Japanese Patent Application Publication No. 2008-069478 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] In the future high-speed transmission of more than 200Gbps, the problem of signal skew (SKEW) is becoming increasingly apparent. The organic fibers described in Patent Documents 1 and 2 can reduce the above-mentioned signal skew problem, but as a base material, prepreg and laminate, there is a problem that sufficient dimensional stability (low warpage) cannot be obtained.

[0011] An object of the present invention is to provide an organic fiber suitable for a fiber cloth serving as a raw material for a laminate satisfying excellent dielectric constant, dielectric loss tangent, and dimensional stability (low warpage).

[0012] Solutions for solving problems

[0013] The gist of the present invention is as follows.

[0014] [1] An organic fiber comprising 5% by mass or more and 100% by mass or less of syndiotactic polystyrene, wherein the organic fiber has a crystallite size of 3 to 10 nm at 2θ=6.8° (110 plane), a crystal orientation degree of 0.92 or more, and a single fiber diameter of 1 to 50 μm.

[0015] [2] The organic fiber according to [1] above, comprising less than 100% by mass of the syndiotactic polystyrene.

[0016] [3] The organic fiber according to [1] or [2], wherein the crystallite size at 2θ=6.8° (110 plane) is 4 to 9 nm.

[0017] [4] The organic fiber according to any one of [1] to [3] above, wherein the degree of crystal orientation at 2θ=20.3° (211 plane) is 0.93 or more, and the crystallization ratio is 0.5 or more.

[0018] [5] The organic fiber according to any one of [1] to [4] above, comprising more than 0% by mass and 95% by mass or less of an amorphous polymer.

[0019] [6] The organic fiber according to [5], comprising 60% by mass or more and 95% by mass or less of the syndiotactic polystyrene and 5% by mass or more and 40% by mass or less of the amorphous polymer.

[0020] [7] The organic fiber according to [5] or [6], wherein the amorphous polymer is polyphenylene ether.

[0021] [8] The organic fiber according to any one of [1] to [7] above, which has a tenacity of 5 or more and 30 or less.

[0022] [9] The organic fiber according to any one of [1] to [8] above, wherein the thermal stress rise temperature is 100° C. to 190° C.

[0023]

[10] The organic fiber according to any one of [1] to [9] above, wherein the thermal expansion coefficient is 300 ppm / °C or less.

[0024]

[11] A prepreg comprising the organic fiber according to any one of [1] to

[10] above and a thermosetting matrix resin composition.

[0025]

[12] A metal-clad laminate comprising a cured product of the prepreg according to

[11] above and a metal foil.

[0026]

[13] A printed wiring board comprising a cured product of the prepreg described in

[11] above.

[0027]

[14] An electronic device comprising the printed circuit board described in

[13] above.

[0028] Effects of the Invention

[0029] According to the present invention, it is possible to provide an organic fiber suitable for a fiber cloth which is a raw material for a laminated board satisfying excellent dielectric constant, dielectric loss tangent, and dimensional stability (low warpage). BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is an example of a wide-angle X-ray two-dimensional scattering pattern of the organic fiber according to the present embodiment.

[0031] Figure 2 This is an example of a circular average profile of wide-angle X-ray scattering of the organic fiber according to the present embodiment.

[0032] It should be noted that Figure 2 The vertical axis is the scattering intensity (arbitrary unit). Figure 2 The horizontal axis is the scattering angle 2θ (unit: °). DETAILED DESCRIPTION

[0033] Hereinafter, a method for implementing the present invention (hereinafter referred to as "this embodiment") will be described. The following embodiment is one method of the present invention, and therefore, the present invention is not limited to the following embodiment. Therefore, the following embodiment can be implemented by appropriately deforming within the scope of the gist of the present invention.

[0034] In addition, "to" in the present application means that the numerical values ​​at both ends are included as the upper limit and the lower limit unless otherwise specified. In the present application, the upper limit and the lower limit of the numerical range can be arbitrarily combined.

[0035] Figure 1 This is an example of a wide-angle X-ray two-dimensional scattering pattern of the organic fiber of this embodiment. Figure 2 This is an example of the circular average profile of wide-angle X-ray scattering of the organic fiber of the present embodiment. In one embodiment, the crystallite size of the organic fiber of the present embodiment at 2θ=6.8° (110 plane) measured by wide-angle X-ray diffraction is 3 to 10 nm, preferably 4 to 9 nm or 5 to 8 nm.

[0036] If the crystallite size at 2θ=6.8° (110 plane) is 3 nm or more, the thermal dimensional stability is good and the dimensional change when the substrate is made is small. If the raw material resin and spinning conditions are set so that the crystallite size at 2θ=6.8° (110 plane) is 10 nm or less, the spinnability is good and the fuzzing can be suppressed, thereby improving the weavability.

[0037] The crystallite size at 2θ=6.8° (110 plane) indicating a crystal structure parallel to the fiber axis is an indicator of thermal dimensional stability. By setting the crystallite size at 2θ=6.8° (110 plane) to be within a specific range, a predetermined effect can be obtained.

[0038] In addition, the crystallite size of the organic fiber of this embodiment at 2θ=6.8° (110 plane) is measured by the method described in Examples.

[0039] Means for controlling the crystallite size of 2θ=6.8° (110 plane) include: setting the resin composition to a specific range, especially increasing the content of amorphous polymer in the resin composition (in one embodiment, the content of amorphous polymer is 5% by mass or more in 100% by mass of the resin composition); setting the spinning conditions (in one embodiment, the spinning temperature, cooling temperature, spinning speed, the amount of crystallization nucleating agent added, etc.) and stretching conditions (in one embodiment, the stretching temperature, stretching ratio, heat setting temperature, relaxation rate, etc.) to a specific range; and reducing the single filament diameter (in one embodiment, the single filament diameter is less than 16 μm), etc.

[0040] It should be noted that even when the resin composition does not contain an amorphous polymer, for example, as spinning conditions, by combining cooling with cold air below 30°C just after ejection and accelerating the spinning speed (in one embodiment, to more than 1000 m / min), the crystallite size can be set to 3 to 10 nm.

[0041] In one embodiment, the degree of crystal orientation of the organic fiber of the present embodiment at 2θ=6.8° (110 plane) measured by wide-angle X-ray diffraction is 0.92 or more, preferably 0.93 or more, 0.94 or more, or 0.95 or more. When the degree of crystal orientation is 0.92 or more, the strength of the organic fiber becomes good.

[0042] The crystal orientation degree of 2θ=6.8° (110 plane) is an index of thermal dimensional stability. By making the crystal orientation degree of 2θ=6.8° (110 plane) fall within a specific range, a predetermined effect can be obtained.

[0043] It should be noted that the degree of crystal orientation of the organic fiber of this embodiment at 2θ=6.8° (110 plane) can be determined according to the azimuth angle range corresponding to the target crystal plane (see Figure 1 The calculation is performed based on the data of the azimuth dependence within the arc arrow in FIG. 1 . More specifically, the measurement is performed using the method described in the examples.

[0044] Means for controlling the degree of crystal orientation of 2θ=6.8° (110 plane) include: setting the resin composition to a specific range (in one embodiment, the content of the amorphous polymer is 40% by mass or less in 100% by mass of the resin composition); setting the spinning conditions and stretching conditions to a specific range, especially increasing the heat setting temperature (in one embodiment, to 130°C or more), etc.

[0045] In one embodiment, the degree of crystal orientation of the organic fiber of the present embodiment at 2θ=20.3° (211 plane) measured by wide-angle X-ray diffraction is preferably 0.93 or more, more preferably 0.94 or more. If the degree of crystal orientation at 2θ=20.3° (211 plane) is 0.93 or more, the strength and thermal dimensional stability of the organic fiber become good.

[0046] The crystal orientation degree of 2θ=20.3° (211 plane) indicating a crystal structure perpendicular to the fiber axis is an indicator of thermal dimensional stability. By setting the crystal orientation degree of 2θ=20.3° (211 plane) in a specific range, a predetermined effect can be obtained.

[0047] In addition, the crystal orientation degree of 2θ=20.3° (211 plane) of the organic fiber of the present embodiment is measured by the method described in Examples.

[0048] Means for controlling the degree of crystal orientation of 2θ=20.3° (211 plane) include: setting the resin composition to a specific range (in one embodiment, the content of amorphous polymer is 40% by mass or less in 100% by mass of the resin composition); setting the spinning conditions and stretching conditions to a specific range, especially increasing the stretching ratio (in one embodiment, to be greater than 1.1), etc.

[0049] In one embodiment, the organic fiber of the present embodiment preferably has a crystallization ratio of 2θ=20.3° (211 plane) measured by wide-angle X-ray diffraction of 0.5 or more. If the crystallization ratio of 2θ=20.3° (211 plane) is 0.5 or more, the crystallized part having excellent thermal dimensional stability is sufficiently increased compared to the amorphous part, and therefore, there is a tendency for the thermal dimensional stability of the organic fiber to become good.

[0050] In addition, the crystallization ratio of 2θ=20.3° (211 plane) of the organic fiber of the present embodiment can be measured by the method described in Examples.

[0051] Means for controlling the crystallization ratio of 2θ=20.3° (211 plane) include: setting the resin composition to a specific range (in one embodiment, the content of the amorphous polymer is 40% by mass or less in 100% by mass of the resin composition); setting the spinning conditions and stretching conditions to a specific range, especially increasing the heat setting temperature (in one embodiment, to 130°C or more), etc.

[0052] In one embodiment, the organic fiber of the present embodiment having a crystal orientation degree of 2θ=20.3° (211 plane) of 0.93 or more and a crystallization ratio of 0.5 or more has good organic fiber strength, thermal dimensional stability, and weavability.

[0053] In one embodiment, the organic fiber of the present embodiment contains 5 mass % or more, preferably 50 mass % or more or 60 mass % or more of syndiotactic polystyrene (hereinafter referred to as sPS) in 100 mass % of the organic fiber of the present embodiment.

[0054] In one embodiment, the organic fiber of the present embodiment contains 100 mass % or less, preferably 95 mass % or less, 90 mass % or less, or 85 mass % or less of sPS in 100 mass % of the organic fiber of the present embodiment.

[0055] When the organic fiber contains 5 mass % or more of sPS, the solvent resistance, dielectric constant and dielectric loss tangent are excellent. In addition, the glass transition temperature of sPS is as low as about 100°C, so from the viewpoint of improving heat resistance, the sPS content is preferably low.

[0056] The syndiotactic polystyrene resin used for the organic fiber of the present embodiment is a styrene-based polymer mainly having a syndiotactic structure.

[0057] Here, the syndiotactic structure means that the stereochemical structure has a syndiotactic structure, that is, a stereo structure in which the phenyl groups as the side chains are alternately located in opposite directions relative to the main chain formed by carbon-carbon bonds, and its stereoregularity is determined by a nuclear magnetic resonance method based on isotopic carbon ( 13 C-NMR method) for analysis.

[0058] use 13The stereoregularity measured by C-NMR method can be expressed by the existence ratio of a plurality of continuous structural units, for example, in the case of 2, it can be expressed by a dyad, in the case of 3, it can be expressed by a triad, and in the case of 5, it can be expressed by a pentad. In a general manner, a polystyrene resin having a syndiotactic structure can have a syndiotacticity of 75% or more, preferably 85% or more, with respect to a racemic dyad, or a syndiotacticity of 30% or more, preferably 50% or more, with respect to a racemic pentad.

[0059] The weight average molecular weight of syndiotactic polystyrene is preferably 30,000 to 500,000. When the weight average molecular weight of sPS is 30,000 or more, the heat resistance and chemical solution resistance required for the substrate become good. When the weight average molecular weight of sPS is 500,000 or less, the extrusion moldability during spinning becomes good.

[0060] The weight average molecular weight of sPS is more preferably 100,000 to 400,000 or 100,000 to 300,000.

[0061] In one embodiment, the organic fiber of the present embodiment contains more than 0 mass %, preferably 5 mass % or more of the amorphous polymer in 100 mass % of the organic fiber of the present embodiment.

[0062] In one embodiment, the organic fiber of the present embodiment contains 95% by mass or less, preferably 40% by mass or less of an amorphous polymer in 100% by mass of the organic fiber of the present embodiment. Since sPS has a fast crystallization rate, the spinnability is improved by including an amorphous polymer that delays crystallization, and the spinning speed can be increased.

[0063] Examples of the amorphous polymer include polyphenylene ether, polyamideimide, polyetherimide, polyethersulfone, polysulfone, and polyarylate.

[0064] In the present application, "amorphous" means a property in which only a glass transition temperature is observed and no melting point exists.

[0065] In one embodiment, the organic fiber of the present embodiment contains 60 mass % to 95 mass % of sPS and 5 mass % to 40 mass % of amorphous polymer in 100 mass % of the organic fiber of the present embodiment, and preferably contains 70 mass % to 85 mass % of sPS and 15 mass % to 30 mass % of amorphous polymer.

[0066] By making the organic fiber of this embodiment contain 60 mass % or more and 95 mass % or less of sPS and 5 mass % or more and 40 mass % or less of amorphous polymer, the dielectric constant and dielectric loss tangent of the organic fiber become sufficiently low values, the heat resistance is also improved, and the spinnability is also good.

[0067] In one embodiment, the organic fiber of the present embodiment preferably contains polyphenylene ether (hereinafter referred to as PPE) as an amorphous polymer. The glass transition temperature of PPE is as high as about 220° C. Therefore, the thermal dimensional stability of the organic fiber is improved by containing PPE.

[0068] In addition, since PPE has low dielectric constant and dielectric loss tangent, when used as a matrix resin of a substrate, the organic fibers containing PPE in the prepreg have high affinity with the matrix resin.

[0069] PPE contains a phenylene ether unit as a repeating structural unit. The phenylene group in the phenylene ether unit may or may not have a substituent.

[0070] PPE may also contain other structural units in addition to the phenylene ether unit. The amount of other structural units relative to the number of all unit structures is typically 30% or less, 25% or less, 20% or less, 15% or less, 10% or less, or 5% or less. However, the amount of other structural units relative to the number of all unit structures may exceed 30% as long as the effect of the present embodiment is not impaired.

[0071] Specific examples of PPE include poly(2,6-dimethyl-1,4-phenylene oxide), poly(2-methyl-6-ethyl-1,4-phenylene oxide), poly(2-methyl-6-phenyl-1,4-phenylene oxide), poly(2,6-dichloro-1,4-phenylene oxide), copolymers of 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol, 2-methyl-6-butylphenol, etc.), and PPE copolymers obtained by coupling 2,6-dimethylphenol with bisphenols or bisphenols.

[0072] The number average molecular weight of PPE is preferably 9000 to 21000. When the number average molecular weight of PPE is 9000 or more, the heat resistance required for the substrate and the chemical solution resistance to the matrix resin composition varnish solvent and the substrate cleaning liquid become good. When the number average molecular weight of PPE is 21000 or less, the extrusion moldability when preparing the resin composition containing PPE and when spinning becomes good.

[0073] The number average molecular weight of PPE is more preferably 9500 or more or 10000 or more. The number average molecular weight of PPE is more preferably 17000 or less or 16000 or less.

[0074] It should be noted that the number average molecular weight and weight average molecular weight of PPE and sPS in the present application are respectively measured by gel permeation chromatography (hereinafter referred to as GPC), and are calculated according to the relationship between the molecular weight and elution time of a standard polystyrene sample measured under the same conditions, and converted to standard polystyrene.

[0075] In one embodiment, the PPE preferably includes or consists of a combination of a PPE component having a number average molecular weight of 9000 to 12000 and a PPE component having a number average molecular weight of 14000 to 17000. This improves both heat resistance and moldability of the organic fiber of the present embodiment.

[0076] The ratio of the PPE component having a number average molecular weight of 9,000 to 12,000 to the PPE component having a number average molecular weight of 14,000 to 17,000 is preferably 20:80 to 80:20.

[0077] In particular, by adjusting the content of the PPE component having a number average molecular weight of 9,000 to 12,000 to 30 to 60% by mass relative to 100% by mass of PPE, both heat resistance and moldability can be further improved, and the affinity between the resin fiber sheet and the matrix resin composition varnish is improved when preparing the prepreg, thereby improving the heat resistance and adhesion of the laminate.

[0078] The number average molecular weight of the PPE component having a number average molecular weight of 9,000 to 12,000 is more preferably 9,500 or more or 10,000 or more, and may be 11,500 or less or 11,000 or less.

[0079] The number average molecular weight of the PPE component having a number average molecular weight of 14,000 to 17,000 is more preferably 14,500 or more or 15,000 or more, and may be 16,500 or less or 16,000 or less.

[0080] In one embodiment, the diameter of the monofilament of the organic fiber of this embodiment (in one embodiment, the monofilament constituting the multifilament) is 1 to 50 μm, preferably 3 to 20 μm or 4 to 16 μm. If the monofilament diameter is too small, there is a tendency that the monofilament strength becomes weak, and the monofilament breaks frequently during spinning and post-processing, which hinders production. If the monofilament diameter is too large, there is a tendency that air cooling cannot be used for cooling during spinning, and the yarn breaks frequently.

[0081] When the monofilament diameter is 1 μm or more, the necessary tensile strength is exhibited in the weaving process and the fiber opening process, and fuzzing (single filament breakage) is not easily generated. When the monofilament diameter is 50 μm or less, the thickness generally sought in substrate applications can be achieved, and in particular, when the monofilament diameter is 30 μm or less, a thickness of 30 to 100 μm suitable for substrate applications can be achieved.

[0082] In one embodiment, the number of monofilaments constituting the multifilament is 10 to 500, preferably 10 to 200, 10 to 100 or 10 to 50. When the number of monofilaments constituting the multifilament is 10 or more, the dielectric constant of the insulating layer of the substrate can be made uniform by adjusting the weaving process and the fiber opening process, and when the number of monofilaments constituting the multifilament is 500 or less, the above-mentioned fuzzing (single filament breakage) is less likely to occur.

[0083] In addition, the single-filament diameter of this embodiment can be measured by the method described in the Example.

[0084] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and 100 mass % or less of syndiotactic polystyrene, has a crystallite size of 3 to 10 nm at 2θ=6.8° (110 plane), a crystal orientation degree of 0.92 or more, and a single fiber diameter of 1 to 50 μm.

[0085] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and less than 100 mass % of syndiotactic polystyrene, has a crystallite size of 3 to 10 nm at 2θ=6.8° (110 plane), a crystal orientation degree of 0.92 or more, and a single fiber diameter of 1 to 50 μm.

[0086] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and 100 mass % or less of syndiotactic polystyrene, has a crystallite size of 4 to 9 nm at 2θ=6.8° (110 plane), a crystal orientation degree of 0.92 or more, and a single fiber diameter of 1 to 50 μm.

[0087] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and less than 100 mass % of syndiotactic polystyrene, has a crystallite size of 4 to 9 nm at 2θ=6.8° (110 plane), a crystal orientation degree of 0.92 or more, and a single fiber diameter of 1 to 50 μm.

[0088] In one embodiment, the organic fiber of the present embodiment preferably contains more than 5 mass% and less than 100 mass% of isotactic polystyrene, the crystallite size at 2θ=6.8° (110 plane) is 3 to 10 nm, the crystal orientation degree is more than 0.92, the crystal orientation degree at 2θ=20.3° (211 plane) is more than 0.93, the crystallization ratio is more than 0.5, and the single fiber diameter is 1 to 50 μm.

[0089] In one embodiment, the organic fiber of the present embodiment preferably contains more than 5 mass% and less than 100 mass% of isotactic polystyrene, the crystallite size at 2θ=6.8° (110 plane) is 3 to 10 nm, the crystal orientation degree is more than 0.92, the crystal orientation degree at 2θ=20.3° (211 plane) is more than 0.93, the crystallization ratio is more than 0.5, and the single fiber diameter is 1 to 50 μm.

[0090] In one embodiment, the organic fiber of the present embodiment preferably contains more than 5 mass% and less than 100 mass% of isotactic polystyrene, the crystallite size at 2θ=6.8° (110 plane) is 4 to 9 nm, the crystal orientation degree is more than 0.92, the crystal orientation degree at 2θ=20.3° (211 plane) is more than 0.93, the crystallization ratio is more than 0.5, and the single fiber diameter is 1 to 50 μm.

[0091] In one embodiment, the organic fiber of the present embodiment preferably contains more than 5 mass% and less than 100 mass% of isotactic polystyrene, the crystallite size at 2θ=6.8° (110 face) is 4 to 9 nm, the crystal orientation degree is more than 0.92, the crystal orientation degree at 2θ=20.3° (211 face) is more than 0.93, the crystallization ratio is more than 0.5, and the single fiber diameter is 1 to 50 μm.

[0092] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and less than 100 mass % of isotactic polystyrene and more than 0 mass % and less than 95 mass % of an amorphous polymer, the crystallite size of 2θ=6.8° (110 plane) is 3 to 10 nm, the crystal orientation degree is greater than 0.92, and the single fiber diameter is 1 to 50 μm.

[0093] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and less than 100 mass % of isotactic polystyrene and more than 0 mass % and less than 95 mass % of an amorphous polymer, the crystallite size at 2θ=6.8° (110 plane) is 4 to 9 nm, the crystal orientation degree is greater than 0.92, and the single fiber diameter is 1 to 50 μm.

[0094] In one embodiment, the organic fiber of the present embodiment preferably contains more than 60 mass % and less than 95 mass % of isotactic polystyrene and more than 5 mass % and less than 40 mass % of amorphous polymer, the crystallite size at 2θ=6.8° (110 plane) is 3 to 10 nm, the crystal orientation degree is more than 0.92, and the single fiber diameter is 1 to 50 μm.

[0095] In one embodiment, the organic fiber of the present embodiment preferably contains more than 60 mass % and less than 95 mass % of isotactic polystyrene and more than 5 mass % and less than 40 mass % of amorphous polymer, the crystallite size at 2θ=6.8° (110 plane) is 4 to 9 nm, the crystal orientation degree is more than 0.92, and the single fiber diameter is 1 to 50 μm.

[0096] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and less than 100 mass % of isotactic polystyrene and more than 0 mass % and less than 95 mass % of polyphenylene ether as an amorphous polymer, the crystallite size of 2θ=6.8° (110 plane) is 3 to 10 nm, the crystal orientation degree is greater than 0.92, and the single fiber diameter is 1 to 50 μm.

[0097] In one embodiment, the organic fiber of the present embodiment preferably contains 5 mass % or more and less than 100 mass % of isotactic polystyrene and more than 0 mass % and less than 95 mass % of polyphenylene ether as an amorphous polymer, the crystallite size at 2θ=6.8° (110 plane) is 4 to 9 nm, the crystal orientation degree is greater than 0.92, and the single fiber diameter is 1 to 50 μm.

[0098] In one embodiment, the tenacity of the organic fiber of the present embodiment is 5 or more and 30 or less. From the viewpoint of weavability, the tenacity of the organic fiber of the present embodiment is preferably 5 or more, 7 or more, or 8 or more. From the viewpoint of spinnability of the raw yarn, the tenacity of the organic fiber of the present embodiment is preferably 30 or less, 20 or less, 17 or less, 15 or less, or 13 or less.

[0099] It should be noted that the toughness is a value measured by the method described in the section [Examples] of the present application.

[0100] In one embodiment, the thermal stress rise temperature of the organic fiber of the present embodiment is preferably 100° C. to 190° C. From the viewpoint of heat resistance and thermal dimensional stability, the thermal stress rise temperature of the organic fiber of the present embodiment is preferably 100° C. or more, 120° C. or more, or 130° C. or more.

[0101] In one embodiment, from the viewpoint of the toughness of the raw yarn, the thermal stress rise temperature of the organic fiber of the present embodiment is preferably 190° C. or lower, 180° C. or lower, 170° C. or lower, or 160° C. or lower.

[0102] It should be noted that the thermal stress rise temperature is the temperature of the inflection point at which stress rises, and if the thermal stress rise temperature is high, the thermal dimensional stability is improved. The thermal stress rise temperature is measured by the method described in the [Examples] section of the present application.

[0103] In one embodiment, the thermal expansion coefficient of the organic fiber of this embodiment is preferably 300 ppm / °C or less, more preferably 200 ppm / °C or less. The thermal expansion coefficient is directly related to the dimensional stability of printed circuit boards, etc., so it is preferably low, and 300 ppm / °C or less is a usable level.

[0104] In addition, from the viewpoint of improving the subsequent weaving process efficiency by increasing the toughness of the fiber and suppressing the breakage of the single yarn, the thermal expansion coefficient of the organic fiber of the present embodiment is preferably 100 ppm / °C or more.

[0105] It should be noted that the thermal expansion coefficient of the organic fiber of the present embodiment can be measured by the method described in the examples.

[0106] In one embodiment, the organic fiber of the present embodiment may contain additional components such as a liquid crystal polyester, a styrene-based elastomer, a flame retardant, an antioxidant, an oil agent, and other additives in addition to sPS, as necessary.

[0107] Liquid crystal polyester (hereinafter also referred to as LCP) includes repeating structural units derived from, for example, aromatic diol, aromatic dicarboxylic acid, and aromatic hydroxycarboxylic acid, and its chemical composition is not particularly limited within the range not impairing the effects of the present embodiment.

[0108] Furthermore, the liquid crystal polyester may include a structural unit derived from an aromatic diamine, an aromatic hydroxyamine, an aromatic aminocarboxylic acid, or the like, within a range not impairing the effects of the present embodiment.

[0109] The melting point of the liquid crystal polyester is preferably 200 to 400°C. When the melting point of the liquid crystal polyester is 200°C or higher, the heat resistance and chemical solution resistance required for the substrate become good. When the melting point of the liquid crystal polyester is 400°C or lower, the extrusion moldability when preparing a resin composition containing PPE and when spinning and the orientation during spinning become good. The melting point of the liquid crystal polyester is more preferably 200 to 380°C or 210 to 350°C.

[0110] The styrene-based elastomer is preferably at least one selected from the group consisting of a styrene-butadiene block copolymer, a styrene-ethylene-butadiene block copolymer, a styrene-ethylene-butylene block copolymer, a styrene-butadiene-butylene block copolymer, a styrene-isoprene block copolymer, a styrene-ethylene-propylene block copolymer, a styrene-isobutylene block copolymer, a hydrogenated product of a styrene-butadiene block copolymer, a hydrogenated product of a styrene-ethylene-butadiene block copolymer, a hydrogenated product of a styrene-butadiene-butylene block copolymer, a hydrogenated product of a styrene-isoprene block copolymer and a styrene homopolymer (polystyrene), and more preferably a hydrogenated product of a styrene-butadiene block copolymer.

[0111] The flame retardant may be any known flame retardant, such as inorganic flame retardants such as antimony trioxide, aluminum hydroxide, magnesium hydroxide, and zinc borate.

[0112] Aromatic bromine compounds such as hexabromobenzene, decabromodiphenylethane, 4,4-dibromobiphenyl, and ethylenebistetrabromophthalimide;

[0113] Phosphorus-based flame retardants such as resorcinol bis(diphenyl phosphate) and resorcinol bis(bis-xylyl phosphate) etc. These flame retardants may be used alone or in combination of two or more.

[0114] In one embodiment, the total content of the additional components in 100% by mass of the organic fiber of the present embodiment is 0 to 20% by mass, preferably 0 to 15% by mass, 0 to 10% by mass, or 0 to 5% by mass.

[0115] The sPS resin composition (hereinafter also referred to as fiber resin) can be prepared by melt-kneading the above-mentioned raw materials such as sPS at, for example, 300° C. or higher using a twin-screw extruder or the like.

[0116] Furthermore, multifilament fibers can be produced from the sPS resin composition by a general spinning method. The spinning conditions include spinning temperature and spinning speed.

[0117] Specifically, by using, for example, a melt spinning method, at a spinning temperature of 280°C or higher, the sPS resin composition is passed through a spinneret (in one embodiment, the hole diameter is 0.23 mm and the number of holes is 24) with a surface temperature heated to 280°C or higher, extruded and spun, thereby producing multifilament fibers.

[0118] The spinning temperature is preferably 285 to 315°C.

[0119] The optimum value of the spinning speed varies depending on the resin composition. For example, in a composition having an sPS content of 50 to 95% by mass and a PPE content of 5 to 50% by mass, the spinning speed is preferably 1000 to 4000 m / min.

[0120] When the spinning speed is 1000 m / min or more, the tenacity becomes good. On the other hand, when the spinning speed is 4000 m / min or less, the decrease in tenacity and the breakage of the yarn are small.

[0121] In the composition where the sPS content is 60 to 90% by mass and the PPE content is 10 to 40% by mass, the spinning speed is more preferably 1500 to 3500 m / min.

[0122] In addition, it is preferred to further stretch the fiber obtained by spinning from the viewpoint of improving toughness and thermal dimensional stability (increasing the thermal stress rise temperature). Stretching may be a process different from spinning, or may be a spin-draw take-up method (Spin-Draw Take-UP Method) in which spinning stretching is performed continuously. Stretching conditions include stretching temperature (in one embodiment, the residual heat temperature of stretching), stretching ratio (in one embodiment, the elongation of the stretched yarn), heat setting temperature (in one embodiment, the heat setting temperature after stretching), and relaxation rate.

[0123] From the viewpoint of quality such as fuzzing and yarn breakage, the elongation of the drawn yarn is preferably 15 to 40%, more preferably 20 to 35%. The drawing ratio is preferably adjusted so as to achieve the above-mentioned elongation.

[0124] The preheating temperature for stretching is preferably 90 to 120° C. When the preheating temperature for stretching is 90° C. or higher, the fiber breakage and single fiber breakage of the organic fiber are less likely to occur. In addition, when the preheating temperature for stretching is 120° C. or lower, the toughness of the organic fiber is less likely to decrease.

[0125] The heat setting temperature after stretching is preferably 120 to 180° C. When the heat setting temperature after stretching is 120° C. or higher, the thermal stress rise temperature of the organic fiber is unlikely to decrease, and when the heat setting temperature after stretching is 180° C. or lower, the toughness of the organic fiber is unlikely to decrease. The heat setting temperature is more preferably 130 to 170° C.

[0126] The relaxation rate is preferably 1 to 20%.

[0127] In addition, the winding tension after heat setting is preferably 0.1 to 0.3 cN / dtex. When the winding tension after heat setting is 0.1 cN / dtex or more, the yarn breakage is less likely to occur during winding. In addition, when the winding tension after heat setting is 0.3 cN / dtex or less, the thermal stress rise temperature is less likely to decrease. A further preferred range of the winding tension after heat setting is 0.15 to 0.25 cN / dtex. In the present application, the winding tension after heat setting is the tension measured on the upper part of the guide just before being wound onto the winding machine.

[0128] The organic fiber of this embodiment can be suitably used for the fiber cloth that becomes the raw material of laminated board.In addition, the organic fiber of this embodiment can be suitably used for the purpose of forming the insulating layer of printed circuit board or the purpose of forming the build-up layer of printed circuit board (that is, the wiring layer of the substrate when the printed circuit board is a build-up substrate).

[0129] Another embodiment of the present invention is a prepreg including the organic fiber of this embodiment and a thermosetting matrix resin composition.

[0130] The thermosetting matrix resin composition may include at least one thermosetting resin selected from the group consisting of epoxy resins, cyanate resins, bismaleimide resins, polyphenylene ether resins, and bismaleimide-triazine resins (BT resins).

[0131] The prepreg of the present embodiment can be produced by, for example, impregnating or coating the organic fiber of the present embodiment with a thermosetting matrix resin composition and then heating and drying the composition.

[0132] The temperature and time of heat drying are not particularly limited, but can be set to, for example, 50 to 200° C. and 1 to 30 minutes from the viewpoint of productivity.

[0133] Another embodiment of the present invention is a metal-clad laminate (hereinafter also referred to as a laminate) including a cured product of the prepreg according to the present embodiment and a metal foil.

[0134] Examples of the metal foil include aluminum foil and copper foil.

[0135] The metal-clad laminate of the present embodiment can be produced by, for example, placing a metal foil on one or both surfaces of the prepreg of the present embodiment and then performing heat-pressing molding.

[0136] Usually, the prepreg is cured by the heat and pressure molding, and the metal-clad laminate of the present embodiment can be obtained.

[0137] In the heat and pressure molding, only one prepreg may be used, or two or more prepregs may be laminated.

[0138] The heat-pressing molding can be performed by, for example, multi-stage pressing, multi-stage vacuum pressing, continuous molding, and an autoclave molding machine.

[0139] The conditions for the heat-pressing molding are not particularly limited, and may be, for example, a temperature of 100 to 300° C., a time of 10 to 300 minutes, and a pressure of 1 to 40 kg / cm 2 .

[0140] Another embodiment of the present invention is a printed wiring board including a cured product of the prepreg of this embodiment.

[0141] The printed circuit board of the present embodiment can be manufactured by, for example, forming a conductor circuit on one or more selected from the group consisting of a cured product of the prepreg of the present embodiment and a metal-clad laminate of the present embodiment using a known method. In addition, a multilayer printed circuit board can be manufactured by further performing a multilayer bonding process as required. The conductor circuit can be formed by, for example, appropriately performing a hole opening process, a metal plating process, an etching of a metal foil, etc.

[0142] Another embodiment of the present invention is an electronic device comprising the printed circuit board. As the electronic device of this embodiment, various electronic devices used in electrical products (such as computers, mobile phones, smart phones, digital cameras, and televisions), vehicles (such as automatic motorcycles, cars, trains, ships, and airplanes, etc.) and the like can be exemplified.

[0143] In one embodiment, the dielectric constant of the cloth including the organic fiber of the present embodiment and the metal-clad laminate of the present embodiment at 10 GHz is not particularly limited, but is preferably 2.7 or less, more preferably 2.6 or less, and even more preferably 2.5 or less.

[0144] In addition, the dielectric constants of the cloth containing organic fibers of the present embodiment and the metal-clad laminate of the present embodiment at 10 GHz were measured by the method described in Examples.

[0145] In one embodiment, the dielectric loss tangent of the cloth including the organic fiber of the present embodiment at 10 GHz is not particularly limited, but is preferably 0.001 or less, more preferably 0.0008 or less, and even more preferably 0.0006 or less.

[0146] In one embodiment, the dielectric loss tangent of the metal-clad laminate of the present embodiment at 10 GHz is not particularly limited, but is preferably 0.0025 or less, more preferably 0.0020 or less, and even more preferably 0.0015 or less.

[0147] In addition, the dielectric constants of the cloth containing organic fibers of the present embodiment and the metal-clad laminate of the present embodiment at 10 GHz were measured by the method described in the Examples.

[0148] Example

[0149] Hereinafter, the present embodiment will be described in detail with reference to examples, but the present embodiment is not limited to the examples.

[0150] <Preparation of organic fiber resin>

[0151] PPE having a number average molecular weight (Mn) shown in Table 1, sPS or atactic PS (polystyrene) having a weight average molecular weight (Mw) shown in Table 1, were melt-kneaded at 320° C. using a twin-screw extruder according to the blending ratio (weight basis) shown in Table 1 to obtain a resin composition. The materials used are shown below.

[0152] ・PPE (product name: "S202A", manufactured by Asahi Kasei Corporation, Mn: 15,000)

[0153] ・PPE (product name "S203A", manufactured by Asahi Kasei Corporation, Mn: 11,000)

[0154] sPS (product name "60ZC", manufactured by Idemitsu Kosan Co., Ltd., Mw: 250,000)

[0155] sPS (product name "90ZC", manufactured by Idemitsu Kosan Co., Ltd., Mw: 200,000)

[0156] Atactic PS (product name "GPPS680", manufactured by PS JAPAN, Mw: 200,000)

[0157] <Production of organic fibers>

[0158] [Examples 1 to 5, Comparative Examples 1 to 3]

[0159] The resin composition shown in Table 1 was passed through a spinneret for extrusion molding and spinning using a melt spinning machine to produce multifilaments. The spinning temperature was adjusted to 295° C., and the surface temperature of the spinneret was adjusted to 293° C. The hole diameter of the spinneret was set to 0.23 mm, and the number of holes was set to 24. In addition, the appropriate spinning speed varies depending on the resin composition, so the spinning speed was changed as described in Table 1.

[0160] After spinning, the fibers were stretched at a preheating temperature of 100°C and a stretching ratio of 20%, and heat-set at the temperature described in Table 1. Then, the fibers of 46 dtex (fineness) and 24 filaments were wound at a winding tension of 0.15 cN / dtex. Two of the fibers were doubling to finally obtain fibers of 92 dtex and 48 filaments.

[0161] <Evaluation method>

[0162] (1) Weight average molecular weight and number average molecular weight

[0163] Using gel permeation chromatography (GPC), the weight average molecular weight and number average molecular weight of each resin such as sPS were determined by comparison with the elution time of standard polystyrene having a known molecular weight.

[0164] Specifically, after preparing a measurement sample with a sample concentration of 0.2w / vol% (solvent: chloroform), the measurement was performed using HLC-8220GPC (manufactured by Tosoh Corporation) as the measurement device, under the conditions of column: Shodex GPC KF-405LHQ×3 (manufactured by Showa Denko K.K.), eluent: chloroform, injection volume: 20μL, flow rate: 0.3mL / min, column temperature: 40°C, and detector: RI.

[0165] (2) Crystallite size

[0166] Wide-angle X-ray scattering of the fibers of Examples and the like was measured under the following conditions using NANOPIX-SP manufactured by Rigaku Corporation, and the crystallite size was calculated from the data of the fan average (-10°<Φ<10°) at 2θ=6.8° (110 plane).

[0167] X-ray wavelength: 0.154nm

[0168] Optical system: Point Collimation (1st 0.55mmφ, 2nd Open, guard 0.35mmφ)

[0169] Detector: Hypix6000-C (two-dimensional semiconductor detector) Repeatedly shoot 4 images vertically

[0170] Camera length: 96.1mm

[0171] Exposure time: 60s / 1 sample

[0172] Environment around the sample: vacuum

[0173] (3) Crystal orientation

[0174] The wide-angle X-ray scattering of the fiber of the embodiment and the like was measured by the same method as in (2) above, and the crystal orientation degree was calculated from the data of azimuthal angle dependency (5.8°<2θ<7.7°) at 2θ=6.8° (110 plane). In addition, the crystal orientation degree was calculated from the data of azimuthal angle dependency (18.6°<2θ<23.1°) at 2θ=20.3° (211 plane).

[0175] (4) Crystallization ratio

[0176] The wide-angle X-ray scattering of the fibers of Examples etc. was measured by the same method as in (2) above, and the crystallization ratio was calculated from the data of azimuthal angle dependence (18.6°<2θ<23.1°) at 2θ=20.3° (211 plane).

[0177] (5) Single filament diameter

[0178] Using a scanning electron microscope (Hitachi Science Systems Co. SEMEDX3 Type N), 100 random cross-sections of the filaments were photographed, and the single-filament diameters of the fibers of Examples and the like were measured, and the average value was calculated.

[0179] (6) Toughness

[0180] The fiber samples of Examples and the like were measured for tensile strength and elongation in accordance with JIS L1013 (2010), and a tensile strength-elongation curve was drawn.

[0181] The test conditions were as follows: the type of the test machine was a constant elongation type, the clamp interval was 20 cm, and the tensile speed was 20 cm / min. It should be noted that when the tensile strength at the time of cutting was less than the maximum strength, the maximum tensile strength and the elongation at that time were measured. In addition, the product of the square root of the strength (A) and the elongation (B), i.e., the toughness, was calculated.

[0182] Strength (A) = tensile strength at break (cN) / fineness (dtex)

[0183] Elongation (B) = Elongation at break (%)

[0184] Toughness = (A) × {(B)} 1 / 2

[0185] (7) Thermal stress rise temperature

[0186] The thermal stress rise temperature of the fiber samples of Examples etc. was measured using a KE-2S thermal stress tester manufactured by INTEC at a heating rate of 150°C / min. The sample was 0.1 m×2 loops, and the initial tension was fineness (dtex)×0.03 cN.

[0187] (8) Thermal expansion coefficient

[0188] The fiber samples of Examples and the like were measured for dimensional changes in different directions using TMA Q400 (manufactured by TA Instruments) under the following conditions to determine the average thermal expansion coefficient between 100 and 200°C.

[0189] Atmosphere: Nitrogen 100mL / min

[0190] Sample size: 8mm

[0191] Measurement mode: Modulated TMA

[0192] Load: 0.02N

[0193] Temperature range: 30→250℃

[0194] Heating rate: 3℃ / min

[0195] Amplitude: 1.0℃

[0196] Cycle: 300s

[0197] Analysis software: Trios (manufactured by TA Instruments)

[0198] (9) Weavability

[0199] The organic fibers of Examples and the like were subjected to sizing, warping, weaving, degumming, and fiber opening processes, and then a cloth was produced so that the warp and weft weaving density was 30 strands / inch and the thickness was 100 μm.

[0200] The warping process used a partial warping machine and the winding was carried out under the condition of a winding tension of 2g.

[0201] The weaving process was performed using a water jet loom at a weaving width of 150 cm and a weaving speed of 400 rpm.

[0202] The degumming process is carried out using a jet steam soaping machine at 95°C.

[0203] The fiber opening process was performed using a calendar roll at a roll temperature of 100° C., a line pressure of 50 N / mm, and a speed of 5 m / min.

[0204] The number of machine stoppages due to yarn breakage during weaving was relatively evaluated in the present embodiment and comparative example, and was set as good (A): within 10 times / day, acceptable (B): 11 to 19 times / day, and unacceptable (C): more than 20 times / day.

[0205] (10) Dielectric constant and dielectric loss tangent (electrical characteristics, 10 GHz)

[0206] The cloth prepared in the above (9) is impregnated with a resin composition varnish containing PPE as a main component (in one embodiment, the content of PPE is 55% by mass as a solid content in 100% by mass of the resin composition varnish) at a predetermined tension of about 100 N / m, the varnish is scraped off with a slit or the like, and dried at 120°C for 3 minutes to prepare a prepreg.

[0207] Six prepregs were stacked and heated from room temperature at a heating rate of 3°C / min under a pressure of 5 kg / cm 2 After reaching 130°C, the temperature was raised at a rate of 3°C / min while the pressure was 40kg / cm 2 After reaching 200°C, the temperature was maintained at 200°C and the pressure was 40 kg / cm 2The vacuum pressurization was then performed for 60 minutes to produce a laminate (hereinafter referred to as a substrate).

[0208] The dielectric constant and dielectric loss tangent of the substrate and the cloth prepared in (9) above were measured at 10 GHz by a cavity resonance method.

[0209] The measurement was performed using a network analyzer (N5230A, manufactured by Agilent Technologies) and a cavity resonator (Cavity Resornator CP series) manufactured by Kanto Denshi Application Development Co., Ltd. as a measurement device.

[0210] (11) Substrate warpage (dimensional stability)

[0211] Two prepregs prepared in the same manner as in (10) above were stacked to make a laminate, and four random 50 mm square specimens were cut out. The warpage of the four corners of each specimen was measured using a vernier caliper (the one with the larger warpage between the front and back). The average value of the four corners was calculated and used as the substrate warpage.

[0212] The smaller the substrate warpage, the higher the dimensional stability.

[0213] As shown in Table 1, under the conditions shown in Examples, the weavability of the cloth was good, the dielectric constant and the dielectric loss tangent were low, the warpage of the substrate was small, and the dimensional stability was excellent.

[0214] In particular, in Examples 1 to 4 where the crystallite size of 2θ=6.8° (110 plane) is in a more preferred range (4 to 9 nm), the weaving property of the cloth is extremely good, and the dielectric constant and dielectric loss tangent are also extremely low. On the other hand, under the conditions shown in the comparative examples, all of good weaving property, low dielectric constant, low dielectric loss tangent, and low warpage (dimensional stability) of the substrate cannot be achieved.

[0215] [Table 1]

[0216]

Claims

1. An organic fiber comprising 5 mass % or more and 100 mass % or less of syndiotactic polystyrene, wherein the organic fiber has a crystallite size of 3 to 10 nm at 2θ=6.8° (110 plane), a crystal orientation degree of 0.92 or more, and a single fiber diameter of 1 to 50 μm. 2 . The organic fiber according to claim 1 , comprising less than 100% by mass of the syndiotactic polystyrene.

3. The organic fiber according to claim 1 or 2, wherein The crystallite size of 2θ=6.8° (110 plane) is 4 to 9 nm.

4. The organic fiber according to claim 1 or 2, wherein The crystal orientation degree of 2θ=20.3° (211 plane) is 0.93 or more, and the crystallization ratio is 0.5 or more. The organic fiber according to claim 2 , comprising more than 0 mass % and 95 mass % or less of the amorphous polymer. 6 . The organic fiber according to claim 5 , comprising 60% by mass or more and 95% by mass or less of the syndiotactic polystyrene and 5% by mass or more and 40% by mass or less of the amorphous polymer.

7. The organic fiber according to claim 5 or 6, wherein The amorphous polymer is polyphenylene ether. 8 . The organic fiber according to claim 1 , which has a tenacity of 5 or more and 30 or less. 9 . The organic fiber according to claim 1 , wherein the thermal stress rising temperature is 100° C. or higher and 190° C. or lower.

10. The organic fiber according to claim 1 or 2, which has a thermal expansion coefficient of 300 ppm / °C or less.

11. A prepreg comprising the organic fiber according to claim 1 or 2 and a thermosetting matrix resin composition. 12 . A metal-clad laminate comprising a cured product of the prepreg according to claim 11 and a metal foil.

13. A printed circuit board comprising a cured product of the prepreg according to claim 11.

14. An electronic device comprising the printed circuit board according to claim 13.