Preparation method of flexible pressure sensor based on composite piezoelectric film

By introducing chlorofluoroethylene and propylene monomers into the piezoelectric film and adding surface-modified PDA@BTO nanoparticles, the problem of poor toughness and flexibility of existing piezoelectric materials in flexible wearable devices is solved, and high voltage is achieved Composite piezoelectric film with electrical properties and flexibility, suitable for wearable electronic devices.

CN119063882APending Publication Date: 2024-12-03ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410970035.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing piezoelectric materials have problems such as low toughness, poor flexibility and poor wear comfort in flexible wearable equipment applications. The widely used piezoelectric sensor materials are mainly high-performance inorganic piezoelectric materials, which have not met the higher demands. .

Method used

A new composite piezoelectric film is adopted, and its substrate is a quaternary polymer. It introduces chlorofluoroethylene and propylene monomers, and adds surface modified PDA@BTO nanoparticles, which are prepared by ultrasonic dispersion and copolymerization methods to improve the The flexibility and piezoelectric properties of the material.

Benefits of technology

It significantly improves piezoelectric performance and flexibility, reduces dielectric loss, enhances material compatibility and dispersion, and is suitable for wearable electronic devices and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952884100000081
    Figure BDA0004952884100000081
Patent Text Reader

Abstract

The invention relates to the field of sensors, and discloses a preparation method of a flexible pressure sensor based on a composite piezoelectric film. According to the flexible pressure sensor, a novel composite piezoelectric film is adopted, a base material of the novel composite piezoelectric film is a quadripolymer, a chlorofluoroethylene monomer and a propylene monomer are introduced to a traditional bipolymer, and CFE is introduced to further improve electrostrictive strain, reduce the Curie temperature of the material and reduce polarization loss, so that the dipole mobility is improved, and the flexible pressure sensor has the advantages of being simple in structure, low in cost and the like. And a unique relaxation ferroelectric property is induced. Propylene is introduced to improve the flexibility of the material and can be used as a structural defect to adjust the structure and performance of the ferroelectric polymer. PDA-coated BTO nanoparticles are compounded in the composite piezoelectric film, so that the composite piezoelectric film has high piezoelectric property, high dielectric constant and low dielectric loss, and is more environment-friendly. And after the BTO is subjected to surface modification, the compatibility and dispersity between the composite piezoelectric film polymer substrate and the BaTiO3 nanoparticles can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sensors, and in particular to a method for preparing a flexible pressure sensor based on a composite piezoelectric film. Background Art

[0002] Piezoelectric materials are materials that can convert mechanical energy into electrical energy. With people's understanding and research of piezoelectric theory, piezoelectric materials have developed from quartz to barium titanate (BTO) ceramics, lead zirconate titanate (PZT) ceramics, and then to piezoelectric polymers and piezoelectric composites. Common piezoelectric materials can be divided into three categories: inorganic piezoelectric materials, organic piezoelectric materials and composite piezoelectric materials.

[0003] Traditional inorganic piezoelectric materials are mainly perovskite structures, mostly based on semiconductor rigid materials. Their low toughness, poor flexibility, and poor wearing comfort limit their application in flexible wearables. Among organic piezoelectric materials, the main ones are ferroelectric polymers based on vinylidene fluoride (VDF). This material has good piezoelectricity, thermoelectricity, and biocompatibility. At the same time, it is superimposed with the inherent properties of polymers such as light weight, easy processing, durability, and flexibility. It is widely used in medicine and biology. Among them, P(VDF-TrFE) is an ideal material for the development of flexible piezoelectric sensors.

[0004] Although many flexible pressure sensors based on P(VDF-TrFE) films have been reported, although the research on P(VDF-TrFE) is quite mature, it still does not meet the needs of higher-demand applications. The widely used piezoelectric sensor materials are still inorganic piezoelectric materials with high piezoelectric properties. Therefore, it is necessary to improve the flexibility and piezoelectric performance of pressure sensors as much as possible, which is of great significance to the development of wearable electronic devices and other fields. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a flexible pressure sensor based on a composite piezoelectric film. The flexible pressure sensor of the present invention adopts a new composite piezoelectric film, whose substrate is a quaternary polymer, and introduces chlorofluoroethylene monomer and propylene monomer into the traditional binary copolymer. The introduction of CFE is to further improve the electrostrictive strain, reduce the Curie temperature of the material, reduce the polarization loss, thereby improving the dipole mobility and inducing unique relaxed ferroelectric properties. The introduction of propylene is to improve the flexibility of the material, and as a structural defect, the structure and performance of the ferroelectric polymer can be adjusted. The composite piezoelectric film is compounded with PDA@BTO nanoparticles, which has high piezoelectric performance, high dielectric constant and low dielectric loss, and is more environmentally friendly. And after surface modification of BTO, the compatibility and dispersibility between the composite piezoelectric film polymer substrate and BaTiO3 nanoparticles can be significantly improved.

[0006] The specific technical solution of the present invention is: a method for preparing a flexible pressure sensor based on a composite piezoelectric film, comprising the following steps:

[0007] Step 1: Add BaTiO3 nanoparticles (BTO) to tris(hydroxymethyl)aminomethane buffer for ultrasonic dispersion, add dopamine hydrochloride, stir the reaction, centrifuge, wash, and dry to obtain PDA@BTO nanoparticles.

[0008] During the above stirring reaction process, dopamine hydrochloride can self-polymerize by cross-linking with oxygen to form polydopamine (PDA), and due to the strong adhesion ability of dopamine, a highly sticky black polydopamine layer can be formed on the surface of BaTiO3 nanoparticles. After the above surface modification treatment of BaTiO3 nanoparticles, the composite piezoelectric film polymer substrate and BaTiO3 nanoparticles can have better compatibility and dispersibility, thereby improving the piezoelectric performance.

[0009] Step 2: Seal the reactor containing potassium persulfate and water and place it in a liquid nitrogen bath for vacuum degassing; introduce gaseous vinylidene fluoride, trifluoroethylene, chlorofluoroethylene and propylene into the reactor, the gas will liquefy instantly when cooled, and heat for copolymerization; cool, separate, wash and dry to obtain a tetrapolymer.

[0010] The present invention finds that the introduction of propylene segments into the copolymer can increase the flexibility of the polymer, thereby facilitating the application of the composite piezoelectric film in wearable devices. At the same time, the propylene segments, as structural defects, also play an important role in adjusting the structure and performance of the polymer.

[0011] Step 3: Ultrasonic dispersion of PDA@BTO nanoparticles in an organic solvent, adding the quaternary copolymer, stirring, and obtaining a PDA@BTO / P(VDF-TrFE-CFE-P) mixed solution. The PDA@BTO nanoparticles account for 12-18% of the total mass of the PDA@BTO nanoparticles and the quaternary copolymer.

[0012] The present invention finds that the doping amount of PDA@BTO nanoparticles has an impact on the performance of the composite piezoelectric film. The introduction of BaTiO3 brings piezoelectricity superposition to the composite piezoelectric film, and as BaTiO3 increases, the piezoelectricity superposition is also enhanced, so that the overall piezoelectric performance of the composite piezoelectric film is improved. However, as BaTiO3 further increases, when it exceeds the critical value, the internal interface defects brought by BaTiO3 have a greater influence on the pressure resistance of the composite piezoelectric film, and the composite piezoelectric film is easily broken down, causing the piezoelectric performance to decrease. In addition, too much inorganic filler BaTiO3 is not conducive to the flexibility of the piezoelectric film. Therefore, too much or too little doping of PDA@BTO nanoparticles will result in poor piezoelectric performance, and an appropriate amount should be added.

[0013] Step 4: Cast the PDA@BTO / P (VDF-TrFE-CFE-P) mixed solution on the substrate, form a composite film after drying, and anneal the composite film.

[0014] Step 5: The annealed composite film is polarized to obtain a PDA@BTO / P (VDF-TrFE-CFE-P) composite piezoelectric film.

[0015] Step 6: First, use PDMS glue to cover the upper and lower parts of the composite piezoelectric film, and then use polyimide tape to encapsulate it. After assembly, a flexible pressure sensor based on the composite piezoelectric film is obtained.

[0016] The composite piezoelectric film is coated with PDMS glue with good flexibility and toughness. It plays a protective role and can also be used as a buffer layer to stably transfer the deformation generated by external force to the composite piezoelectric film. The outermost layer is the encapsulation layer, and the sensor is encapsulated with PI (polyimide) tape, which is resistant to high temperature, insulated, and highly protective.

[0017] In summary, the flexible pressure sensor of the present invention adopts a new type of composite piezoelectric film, whose substrate is a quaternary polymer, and introduces chlorofluoroethylene (CFE) monomer units and propylene monomer units into the traditional binary copolymer. The introduction of CFE is to further improve the electrostrictive strain, reduce the Curie temperature of the material, reduce the polarization loss, thereby improving the dipole mobility, and inducing a unique relaxed ferroelectric property. Propylene is introduced to improve the flexibility of the material, and as a structural defect, the structure and performance of the ferroelectric polymer can be adjusted. The composite piezoelectric film is compounded with PDA@BTO nanoparticles, which has high piezoelectric performance, high dielectric constant and low dielectric loss, and is more environmentally friendly. And after surface modification of BTO, the compatibility and dispersibility between the composite piezoelectric film polymer substrate and BaTiO3 nanoparticles can be significantly improved.

[0018] Preferably, in step 1, the mass ratio of the BaTiO3 nanoparticles to dopamine hydrochloride is 1:(1-1.5).

[0019] In the process of surface modification of BTO, the hydrogen bonds formed by the interaction between the -NH bonds of PDA and the -CF bonds of the polymer greatly improve the compatibility and dispersibility between the components, significantly reduce the interface pore defects and cracks between BTO and the polymer, thereby improving the performance output of the pressure sensor. However, the amount of dopamine hydrochloride should be appropriate. If it is too much, the BTO surface coating layer will be thicker, which will weaken the effect of BTO. If it is too little, the effect on the dispersibility and compatibility of BTO in the polymer substrate is not obvious, thus affecting the performance of the pressure sensor.

[0020] Preferably, in step 1, the stirring reaction is carried out at a temperature of 20 to 40° C. and for a time of 20 to 30 hours.

[0021] Preferably, in step 2, the molar ratio of vinylidene fluoride, trifluoroethylene, chlorofluoroethylene and propylene is 63-69: 22.5-33.5: 6.5-8.5: 3.5-5.5.

[0022] The present invention finds that the content of propylene monomer needs to be strictly controlled. If its content is too high, its side methyl structure will increase the interlamellar spacing, which is not conducive to the transformation of the polar phase; if its content is too low, it is not conducive to improving the flexibility of the composite piezoelectric film.

[0023] Preferably, in step 2, the copolymerization temperature is 85-95° C. and the time is 4-8 h.

[0024] Preferably, in step three, the organic solvent is N,N-dimethylformamide (DMF).

[0025] Preferably, in step three, the stirring temperature is 45-55° C., the rotation speed is 300-500 r / min, and the time is 2-4 h.

[0026] Preferably, in step 4, the annealing treatment is performed at a temperature of 100 to 110° C. for 8 to 12 hours, and the annealing treatment is followed by cooling to room temperature.

[0027] Within this annealing temperature window, the quaternary copolymer film possesses a nonpolar pure relaxation phase and exhibits a critical transition phenomenon with an extremely small energy barrier between the nonpolar (relaxed) and polar (ferroelectric) condensed chain states, which is favorable for the formation of the β phase.

[0028] Preferably, in step five, the polarization treatment specifically includes: placing the annealed composite film on a tray, connecting the ITO as the lower electrode to the tray with a conductive silver paste for grounding, using silver as the upper electrode, and polarizing the film to obtain a PDA@BTO / P (VDF-TrFE-CFE-P) composite piezoelectric film.

[0029] Preferably, in step five, the polarization electric field is 120-160 MV / m, the polarization temperature is 70-90° C., and the polarization time is 30-50 min.

[0030] Compared with the prior art, the beneficial effects of the present invention are:

[0031] (1) The base material of the composite piezoelectric film in the flexible pressure sensor of the present invention is a quaternary polymer, which is obtained by introducing chlorofluoroethylene monomer and propylene monomer into the traditional binary copolymer. The introduction of CFE is to further increase the electrostrictive strain, reduce the Curie temperature of the material, reduce the polarization loss, thereby increasing the dipole mobility and inducing a unique relaxed ferroelectric property. The introduction of propylene is to improve the flexibility of the material and to adjust the structure and properties of the ferroelectric polymer as a structural defect.

[0032] (2) The composite piezoelectric film of the present invention is compounded with PDA@BTO nanoparticles, has high piezoelectric performance, high dielectric constant and low dielectric loss, and is more environmentally friendly. The surface modification of BTO can significantly improve the compatibility and dispersibility between the polymer substrate of the composite piezoelectric film and the BaTiO3 nanoparticles.

[0033] (3) The piezoelectric properties of the composite piezoelectric film of the present invention are significantly improved, and it also has excellent flexibility, impact resistance and good electrical conductivity and cyclicity, and can be used in the fields of imaging acoustic transducers, motion detection sensors, wearable electronic devices, etc. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0035] Comparative Example 1

[0036] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized (DI) water to a 300ml stainless steel container. The container is sealed and placed in a -140℃ liquid nitrogen bath, and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE) and propylene monomers are pumped into the container in a molar ratio of 63:25:7:5 and liquefied instantly at liquid nitrogen temperature. The reaction is carried out at 90℃ for 6 hours. After the reaction is completed, the container is cooled to room temperature and excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50℃.

[0037] Step 2: Prepare a pure tetrapolymer film by solution casting method, take 1.20g of the above-prepared product and dissolve it in 10ml N,N-dimethylformamide (DMF), stir it magnetically overnight (24h) to obtain a homogeneous solution. Then cast it on a clean glass substrate, dry it in a 60℃ oven for 8h to evaporate the organic solvent, peel off the film after drying and put it into a vacuum oven, adjust the temperature at 110℃ for annealing for 12h, wait for the film to slowly cool to room temperature, and take out the film.

[0038] Step 3: polarize the above-mentioned film, place the composite film obtained in step 2 on a tray, connect the ITO as the lower electrode to the tray with conductive silver paste for grounding, use silver as the upper electrode, and then polarize the film, adjust the polarization electric field to 140MV / m, the polarization temperature to 80°C, and the polarization time to 40min, and then obtain a pure P (VDF-TrFE-CFE-P) piezoelectric film.

[0039] Step 4: Use PDMS glue with good flexibility and toughness to cover the composite piezoelectric film from top to bottom. Use PI (polyimide) tape to encapsulate the sensor on the outermost layer to obtain a flexible piezoelectric sensor.

[0040] Comparative Example 2

[0041] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized (DI) water to a 300ml stainless steel container. The container is sealed and placed in a -140℃ liquid nitrogen bath, and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE) and chlorofluoroethylene (CFE) monomers are pumped into the container at a molar ratio of 63:25:7 and liquefied instantly at liquid nitrogen temperature. The reaction is carried out at 90℃ for 6 hours. After the reaction is completed, the container is cooled to room temperature and excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50℃.

[0042] Step 2: Dissolve 0.05g tris(hydroxymethyl)aminomethane in 40ml deionized water to form a buffer solution, add 0.10g BTO nanoparticles and ultrasonicate for 30min to make it evenly dispersed, then mix 0.12g dopamine hydrochloride in the solution and stir magnetically at room temperature for 24h. During the stirring process, dopamine can self-polymerize by cross-linking with oxygen to form polydopamine (PDA), and due to the strong adhesion ability of dopamine, a highly sticky black polydopamine layer can be formed on the surface of BTO nanoparticles. The PDA@BTO nanoparticles formed by centrifugation were washed 3 times with ethanol aqueous solution. Finally, the resultant was dried in an oven at 60°C for 8 hours to obtain BTO-modified black nanoparticles.

[0043] Step 3: Weigh 0.164g of the prepared PDA@BTO nanoparticles and 1.20g of P(VDF-TrFE-CFE) solid, then disperse 0.164g of PDA@BTO nanoparticles in 20mL of DMF solvent, and then ultrasonicate for 30min to evenly disperse the nanoparticles in DMF solvent. Finally, add 1.20g of P(VDF-TrFE-CFE) solid, stir magnetically for 3h in a 50℃ water bath, and rotate at 400r / min to obtain a uniform PDA@BTO / P(VDF-TrFE-CFE) mixed solution.

[0044] Step 4: Prepare the composite film by solution casting method, cast the prepared solution onto a clean glass substrate, and dry it in a 60°C oven for 2 hours to evaporate the organic solvent to form a composite film. After drying, peel off the film and put it into a vacuum oven, adjust the temperature at 110°C for annealing for 8 hours, wait for the film to slowly cool to room temperature, and take out the film.

[0045] Step 5: polarize the above-mentioned composite film, place the composite film obtained in step 3 on a tray, connect the ITO as the lower electrode to the tray with conductive silver paste for grounding, use silver as the upper electrode, and then polarize the film, adjust the polarization electric field to 140MV / m, the polarization temperature to 80°C, and the polarization time to 40min, and then obtain the PDA@BTO / P(VDF-TrFE-CFE) composite piezoelectric film.

[0046] Step 6: Use PDMS glue with good flexibility and toughness to cover the composite piezoelectric film from top to bottom. Use PI (polyimide) tape to encapsulate the sensor on the outermost layer to obtain a flexible piezoelectric sensor.

[0047] Example 1

[0048] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized (DI) water to a 300ml stainless steel container. The container is sealed and placed in a -140℃ liquid nitrogen bath, and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE) and propylene monomers are pumped into the container in a molar ratio of 63:25:7:5 and liquefied instantly at liquid nitrogen temperature. The reaction is carried out at 90℃ for 6 hours. After the reaction is completed, the container is cooled to room temperature and excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50℃.

[0049] Step 2: Dissolve 0.05g tris(hydroxymethyl)aminomethane in 40ml deionized water to form a buffer solution, add 0.10g BTO nanoparticles and ultrasonicate for 30min to make it evenly dispersed, then mix 0.12g dopamine hydrochloride in the solution and stir magnetically at room temperature for 24h. During the stirring process, dopamine can self-polymerize by cross-linking with oxygen to form polydopamine (PDA), and due to the strong adhesion ability of dopamine, a highly sticky black polydopamine layer can be formed on the surface of BTO nanoparticles. The PDA@BTO nanoparticles formed by centrifugation were washed 3 times with ethanol aqueous solution. Finally, the resultant was dried in an oven at 60°C for 8 hours to obtain BTO-modified black nanoparticles.

[0050] Step 3: Weigh 0.164g of the prepared PDA@BTO nanoparticles and 1.20g of P(VDF-TrFE-CFE-P) solid, then disperse 0.164g of PDA@BTO nanoparticles in 20mL of DMF solvent, and then ultrasonicate for 30min to evenly disperse the nanoparticles in DMF solvent. Finally, add 1.20g of P(VDF-TrFE-CFE-P) solid, stir magnetically for 3h in a 50℃ water bath, and rotate at 400r / min to obtain a uniform PDA@BTO / P(VDF-TrFE-CFE-P) mixed solution.

[0051] Step 4: Prepare the composite film by solution casting method, cast the prepared solution onto a clean glass substrate, and dry it in a 60°C oven for 2 hours to evaporate the organic solvent to form a composite film. After drying, peel off the film and put it into a vacuum oven, adjust the temperature at 110°C for annealing for 8 hours, wait for the film to slowly cool to room temperature, and take out the film.

[0052] Step 5: polarize the above-mentioned composite film, place the composite film obtained in step 3 on a tray, connect the ITO as the lower electrode to the tray with conductive silver paste for grounding, use silver as the upper electrode, and then polarize the film, adjust the polarization electric field to 140MV / m, the polarization temperature to 80°C, and the polarization time to 40min, and then obtain the PDA@BTO / P (VDF-TrFE-CFE-P) composite piezoelectric film.

[0053] Step 6: Use PDMS glue with good flexibility and toughness to cover the composite piezoelectric film from top to bottom. Use PI (polyimide) tape to encapsulate the sensor on the outermost layer to obtain a flexible piezoelectric sensor.

[0054] Example 2

[0055] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized (DI) water to a 300ml stainless steel container. The container is sealed and placed in a -140℃ liquid nitrogen bath, and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE) and propylene monomers are pumped into the container in a molar ratio of 63:25:7:5 and liquefied instantly at liquid nitrogen temperature. The reaction is carried out at 90℃ for 6 hours. After the reaction is completed, the container is cooled to room temperature and excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50℃.

[0056] Step 2: Dissolve 0.05g tris(hydroxymethyl)aminomethane in 40ml deionized water to form a buffer solution, add 0.10g BTO nanoparticles and ultrasonicate for 30min to make it evenly dispersed, then mix 0.12g dopamine hydrochloride in the solution and stir magnetically at room temperature for 24h. During the stirring process, dopamine can self-polymerize by cross-linking with oxygen to form polydopamine (PDA), and due to the strong adhesion ability of dopamine, a highly sticky black polydopamine layer can be formed on the surface of BTO nanoparticles. The PDA@BTO nanoparticles formed by centrifugation were washed 3 times with ethanol aqueous solution. Finally, the resultant was dried in an oven at 60°C for 8 hours to obtain BTO-modified black nanoparticles.

[0057] Step 3: Weigh 0.212g of the prepared PDA@BTO nanoparticles and 1.20g of P(VDF-TrFE-CFE-P) solid, then disperse 0.212g of PDA@BTO nanoparticles in 20mL of DMF solvent, and then ultrasonicate for 30min to evenly disperse the nanoparticles in DMF solvent. Finally, add 1.20g of P(VDF-TrFE-CFE-P) solid, stir magnetically for 3h in a 50℃ water bath, and rotate at 400r / min to obtain a uniform PDA@BTO / P(VDF-TrFE-CFE-P) mixed solution.

[0058] Step 4: Prepare the composite film by solution casting method, cast the prepared solution onto a clean glass substrate, and dry it in a 60°C oven for 2 hours to evaporate the organic solvent to form a composite film. After drying, peel off the film and put it into a vacuum oven, adjust the temperature at 110°C for annealing for 8 hours, wait for the film to slowly cool to room temperature, and take out the film.

[0059] Step 5: polarize the above-mentioned composite film, place the composite film obtained in step 3 on a tray, connect the ITO as the lower electrode to the tray with conductive silver paste for grounding, use silver as the upper electrode, and then polarize the film, adjust the polarization electric field to 140MV / m, the polarization temperature to 80°C, and the polarization time to 40min, and then obtain the PDA@BTO / P (VDF-TrFE-CFE-P) composite piezoelectric film.

[0060] Step 6: Use PDMS glue with good flexibility and toughness to cover the composite piezoelectric film from top to bottom. Use PI (polyimide) tape to encapsulate the sensor on the outermost layer to obtain a flexible piezoelectric sensor.

[0061] Example 3

[0062] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized (DI) water to a 300ml stainless steel container. The container is sealed and placed in a -140℃ liquid nitrogen bath, and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE) and propylene monomers are pumped into the container in a molar ratio of 63:25:7:5 and liquefied instantly at liquid nitrogen temperature. The reaction is carried out at 90℃ for 6 hours. After the reaction is completed, the container is cooled to room temperature and excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50℃.

[0063] Step 2: Dissolve 0.05g tris(hydroxymethyl)aminomethane in 40ml deionized water to form a buffer solution, add 0.10g BTO nanoparticles and ultrasonicate for 30min to make it evenly dispersed, then mix 0.12g dopamine hydrochloride in the solution and stir magnetically at room temperature for 24h. During the stirring process, dopamine can self-polymerize by cross-linking with oxygen to form polydopamine (PDA), and due to the strong adhesion ability of dopamine, a highly sticky black polydopamine layer can be formed on the surface of BTO nanoparticles. The PDA@BTO nanoparticles formed by centrifugation were washed 3 times with ethanol aqueous solution. Finally, the resultant was dried in an oven at 60°C for 8 hours to obtain BTO-modified black nanoparticles.

[0064] Step 3: Weigh 0.263g of the prepared PDA@BTO nanoparticles and 1.20g of P(VDF-TrFE-CFE-P) solid, then disperse 0.263g of PDA@BTO nanoparticles in 20mL of DMF solvent, and then ultrasonicate for 30min to evenly disperse the nanoparticles in DMF solvent. Finally, add 1.20g of P(VDF-TrFE-CFE-P) solid, stir magnetically for 3h in a 50℃ water bath, and rotate at 400r / min to obtain a uniform PDA@BTO / P(VDF-TrFE-CFE-P) mixed solution.

[0065] Step 4: Prepare the composite film by solution casting method, cast the prepared solution onto a clean glass substrate, and dry it in a 60°C oven for 2 hours to evaporate the organic solvent to form a composite film. After drying, peel off the film and put it into a vacuum oven, adjust the temperature at 110°C for annealing for 8 hours, wait for the film to slowly cool to room temperature, and take out the film.

[0066] Step 5: polarize the above-mentioned composite film, place the composite film obtained in step 3 on a tray, connect the ITO as the lower electrode to the tray with conductive silver paste for grounding, use silver as the upper electrode, and then polarize the film, adjust the polarization electric field to 140MV / m, the polarization temperature to 80°C, and the polarization time to 40min, and then obtain the PDA@BTO / P (VDF-TrFE-CFE-P) composite piezoelectric film.

[0067] Step 6: Use PDMS glue with good flexibility and toughness to cover the composite piezoelectric film from top to bottom. Use PI (polyimide) tape to encapsulate the sensor on the outermost layer to obtain a flexible piezoelectric sensor.

[0068] Performance Testing

[0069] The pressure sensors of the comparative example and the embodiment are tested, and the results are shown in the following table:

[0070]

[0071] It can be seen from the data in the above table that after adding PDA@BTO, the performance of the prepared composite piezoelectric film is better than that of the pure tetrapolymer film (Comparative Example 1). The maximum output voltage of the film in Example 1 is 11.28V, and the maximum current density is 336nA. The stability of the film was tested using a cyclic load test device. It was found that after 8800 test cycles, it can still maintain an output voltage of ~10.73V without obvious attenuation, indicating that it has excellent stability. In Example 2, the content of PDA@BTO is increased, and the performance of the prepared composite film is improved. However, it can be seen from Example 3 that the performance begins to decrease as the content of PDA@BTO continues to increase, indicating that for this composite piezoelectric film, the content of PDA@BTO has an optimal ratio.

[0072] In addition, it can be seen from the data results of the embodiment and comparative example 2 that the copolymerized propylene monomer can significantly improve the elongation at break of the composite film, that is, improve the flexibility of the composite film, so that it can be applied to fields such as wearable electronic devices.

[0073] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0074] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a flexible pressure sensor based on a composite piezoelectric film, characterized in that: The following steps are involved: Step 1: Add BaTiO3 nanoparticles to tris(hydroxymethyl)aminomethane buffer for ultrasonic dispersion, add dopamine hydrochloride, stir for reaction, centrifuge, wash, and dry to obtain PDA@BTO nanoparticles; Step 2: Seal the reactor containing potassium persulfate and water and place it in a liquid nitrogen bath for vacuum degassing; introduce gaseous vinylidene fluoride, trifluoroethylene, chlorofluoroethylene and propylene into the reactor, the gas will liquefy instantly when cooled, and heat for copolymerization; cooling, separating, washing and drying to obtain a tetrapolymer; Step 3: ultrasonically dispersing the PDA@BTO nanoparticles in an organic solvent, adding the quaternary copolymer, and stirring to obtain a PDA@BTO / P(VDF-TrFE-CFE-P) mixed solution; the PDA@BTO nanoparticles account for 12-18% of the total mass of the PDA@BTO nanoparticles and the quaternary copolymer; Step 4: casting the PDA@BTO / P(VDF-TrFE-CFE-P) mixed solution on the substrate, forming a composite film after drying, and annealing the composite film; Step 5: polarizing the annealed composite film to obtain a PDA@BTO / P (VDF-TrFE-CFE-P) composite piezoelectric film; Step 6: First, use PDMS glue to cover the upper and lower parts of the composite piezoelectric film, and then use polyimide tape to encapsulate it. After assembly, a flexible pressure sensor based on the composite piezoelectric film is obtained.

2. The preparation method according to claim 1, characterized in that: In step 1, the mass ratio of the BaTiO3 nanoparticles to dopamine hydrochloride is 1:(1-1.5).

3. The preparation method according to claim 1 or 2, characterized in that: In step 1, the stirring reaction is carried out at a temperature of 20 to 40° C. and for a time of 20 to 30 hours.

4. The preparation method according to claim 1, characterized in that: In step 2, the molar ratio of vinylidene fluoride, trifluoroethylene, chlorofluoroethylene and propylene is 63-69: 22.5-33.5: 6.5-8.5: 3.5-5.

5.

5. The preparation method according to claim 1 or 4, characterized in that: In step 2, the copolymerization temperature is 85-95° C. and the time is 4-8 hours.

6. The preparation method according to claim 1, characterized in that: In step 3, the organic solvent is N,N-dimethylformamide.

7. The preparation method according to claim 1, characterized in that: In step 3, the stirring temperature is 45-55° C., the rotation speed is 300-500 r / min, and the time is 2-4 h.

8. The preparation method according to claim 1, characterized in that: In step 4, the annealing treatment is performed at a temperature of 100 to 110° C. for 8 to 12 hours, and then cooled to room temperature.

9. The preparation method according to claim 1, characterized in that: In step five, the polarization treatment specifically includes: placing the annealed composite film on a tray, connecting the ITO as the lower electrode to the tray with a conductive silver paste for grounding, using silver as the upper electrode, polarizing the film to obtain a PDA@BTO / P (VDF-TrFE-CFE-P) composite piezoelectric film.

10. The preparation method according to claim 9, characterized in that: In step 5, the polarization electric field is 120-160 MV / m, the polarization temperature is 70-90° C., and the polarization time is 30-50 min.

Citation Information

Cited By

  • Flexible SiC composite film with in-situ pressure monitoring function and preparation method thereof

    CN119978825A