Method for simultaneously measuring contents of germanium, indium and tin in polymetallic ore

Through sodium peroxide melting method and acid dissolution treatment technology, combined with inductively coupled plasma mass spectrometry, the problem of low-content determination of germanium, indium and tin elements in multimetallic ores is solved, and efficient and accurate multi-element analysis is achieved, reducing impurities Interference, suitable for rapid detection of large batches of samples.

CN119064113APending Publication Date: 2024-12-03GUIZHOU PROVINCIAL GEOLOGICAL & MINERAL RESOURCES CENT LAB
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411205101.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art is difficult to accurately and efficiently determine the content of germanium, indium and tin elements in polymetallic ores simultaneously, especially at low content, and there are instrument background interference and impurities, which cannot meet the needs of rapid detection of large-scale samples.

Method used

The polymetallic ore sample was leaching with ammonium hydroxide-ammonium salt buffer solution and iron hydroxide by sodium peroxide melting method, and precipitating germanium, indium and tin elements through acid dissolution adjustment, and then dissolved and inductively coupled. Plasma mass spectrometry test reduces matrix interference and achieves accurate determination of elements.

Benefits of technology

It realizes efficient and accurate determination of germanium, indium and tin elements in polymetallic ores, reduces impurity interference, is suitable for rapid detection of low-content samples, meets the needs of large-scale sample analysis, and improves the precision and accuracy of detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005018808780000081
    Figure BDA0005018808780000081
  • Figure BDA0005018808780000101
    Figure BDA0005018808780000101
  • Figure BDA0005018808780000111
    Figure BDA0005018808780000111
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical analysis, and particularly relates to a method for simultaneously determining germanium, indium and tin contents in polymetallic ore. The method for simultaneously measuring the contents of germanium, indium and tin in the polymetallic ore comprises the following steps: mixing and melting a polymetallic ore sample and sodium peroxide to obtain a melt; the melt, an ammonium hydroxide-ammonium salt buffer solution and ferric hydroxide are mixed for extraction and then mixed with a first acid solution for acid dissolution, and a mixed solution is obtained; adjusting the pH value of the mixed solution to 9-10, and precipitating to obtain a precipitated solid containing germanium, indium and tin; dissolving the sediment solid containing germanium, indium and tin in a second acid solution to obtain a to-be-detected solution; and carrying out inductively coupled plasma mass spectrometry test on the to-be-tested liquid to obtain the contents of germanium, indium and tin elements in the polymetallic ore. The method can be used for simultaneously detecting the contents of germanium, indium and tin elements in the polymetallic ore, the detection method is efficient, and the detection result is accurate and reliable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical analysis, and in particular relates to a method for simultaneously determining the contents of germanium, indium and tin in a polymetallic ore. Background Art

[0002] The types of rock and mineral samples associated with scattered and non-ferrous metal elements are complex. For example, the scattered elements germanium (Ge), indium (In) and non-ferrous metal tin (Sn) are generally associated with polymetallic ores such as lead-zinc ore, copper ore, zinc ore, tin-lead ore, and often coexist with sulfide ores to form composite polymetallic deposits. However, due to the very low content of scattered elements and non-ferrous metal elements in geological samples, the minerals need to be digested and pre-treated in the process of analyzing the associated ores, and then extracted, separated and enriched to obtain the test solution before being measured on the machine; the process is relatively cumbersome and not suitable for rapid determination of large quantities of samples, especially large geological survey samples.

[0003] In the national standard GB / T8151 series of analytical methods, the detection range (mass fraction) of the determination method of germanium is 0.0005% to 0.10%, and the detection range (mass fraction) of the determination method of indium is 0.0020% to 0.10%. It is impossible to detect germanium below 0.0005% and indium below 0.0020% in minerals, and there is a lack of determination methods for tin. At present, the commonly used analytical method for germanium is atomic fluorescence spectrometry, but this method has certain limitations for the determination of high-content germanium. Due to the narrow linear range, it is necessary to separate the solution, add acid, shake it well and then measure it. Its advantages are obviously insufficient, and the efficiency of single element determination is not high. The commonly used analytical method for indium is inductively coupled plasma mass spectrometry. Since the content of indium in the earth's crust is very low, it has high requirements in terms of pretreatment (ore dissolution) methods and on-machine determination conditions; for tin, AC arc-emission spectrometry is mostly used, but this method is not stable and has poor detection capabilities for trace elements.

[0004] With the advancement of science and technology, the use of inductively coupled plasma mass spectrometers (ICP-MS) with high sensitivity, precision and strong anti-interference ability to analyze minerals has become the mainstream of current geological analysis laboratories. ICP-MS has the advantages of fast analysis speed, high sensitivity, good precision, high accuracy, and wide linear range of determination, and has unique advantages in the analysis of trace elements. However, due to the complexity of geological samples, when ICP-MS directly determines the elements of germanium, indium and tin in geological samples, there is instrument background interference, which directly affects the accuracy of the analysis data. The prior art pre-treats the geological samples to improve the purity of the samples to be tested, such as using a nitric acid-hydrofluoric acid-perchloric acid system to dissolve the samples, adding phosphoric acid to avoid the volatilization loss of germanium, and using atomic fluorescence spectrometry for determination, but the liquid to be tested still contains certain impurities that affect the test results, and the method has a narrow linear range, and the single element determination mode is not conducive to batch detection needs.

[0005] Therefore, there is an urgent need to explore an accurate, efficient and simultaneous analytical method for the determination of germanium, indium and tin elements in polymetallic mineral samples. Summary of the invention

[0006] In view of this, the present invention provides a method for simultaneously determining the content of germanium, indium and tin in a polymetallic ore. The detection method provided by the present invention can efficiently and simultaneously detect the content of germanium, indium and tin elements in a polymetallic ore, and the detection result is accurate and reliable.

[0007] In order to solve the above technical problems, the present invention provides a method for simultaneously determining the content of germanium, indium and tin in a polymetallic ore, comprising the following steps:

[0008] Mixing and melting the polymetallic ore sample and sodium peroxide to obtain a molten material;

[0009] The molten material, the ammonium hydroxide-ammonium salt buffer solution, and the ferric hydroxide are mixed for leaching, and then mixed with the first acid solution for acid dissolution to obtain a mixed solution;

[0010] The pH value of the mixed solution is adjusted to 9-10 for precipitation to obtain a precipitated solid containing germanium, indium and tin;

[0011] Dissolving the precipitated solid containing germanium, indium and tin in a second acid solution to obtain a test solution;

[0012] The test solution is tested by inductively coupled plasma mass spectrometry to obtain the element contents of germanium, indium and tin in the polymetallic ore sample.

[0013] Preferably, the mass ratio of the polymetallic ore sample to sodium peroxide is 0.1-0.2:2.0-3.0.

[0014] Preferably, the melting temperature is 700-800° C. and the melting time is 10-20 min.

[0015] Preferably, the pH value of the ammonium hydroxide-ammonium salt buffer solution is 9.5 to 9.8;

[0016] The volume ratio of the mass of the polymetallic ore sample to the ammonium hydroxide-ammonium salt buffer solution is 0.1-0.2 g:45-55 mL;

[0017] The mass ratio of the polymetallic ore sample to iron hydroxide is 0.1-0.2 g: 5.0-10.0 mg;

[0018] The polymetallic ore samples include germanium-rich lead-zinc ore, copper ore, germanium ore, galena or zinc ore.

[0019] Preferably, the leaching temperature is 98-110° C. and the leaching time is 1.5-2.5 min.

[0020] Preferably, the first acid solution is a nitric acid solution or a hydrochloric acid solution; the mass concentration of the first acid solution is 48-52%.

[0021] Preferably, the second acid solution is a nitric acid solution; the mass concentration of the second acid solution is 45-55%.

[0022] Preferably, the pH regulator used to adjust the pH value of the mixed solution to 9-10 is ammonia water; the mass concentration of the ammonia water is 45-55%.

[0023] Preferably, the test conditions of the inductively coupled plasma mass spectrometry test include:

[0024] The nebulizer was a high-sensitivity concentric nebulizer with a nebulization chamber temperature of 2.70°C;

[0025] RF power is 1550W;

[0026] The carrier gas is argon with a purity greater than 99.99%, and the carrier gas flow rate is 1.05L / min;

[0027] The auxiliary gas flow rate is 0.90L / min;

[0028] The helium flow rate is 5.0 mL / min;

[0029] The peristaltic pump speed is 40 rpm;

[0030] The sampling cone / interceptor cone are both nickel cones, the sampling cone diameter is 1.1mm, and the interceptor cone diameter is 0.5mm; the sampling mode is peak jumping; the sampling depth is 5.0mm; and the number of repetitions is 5 times.

[0031] Preferably, the inductively coupled plasma mass spectrometry test is an internal standard method.

[0032] The present invention provides a method for simultaneously determining the content of germanium, indium and tin in a polymetallic ore, comprising the following steps: mixing and melting a polymetallic ore sample and sodium peroxide to obtain a melt; mixing the melt, ammonium hydroxide-ammonium salt buffer solution and ferric hydroxide for leaching and then mixing with a first acid solution for acid dissolution to obtain a mixed solution; adjusting the pH value of the mixed solution to 9-10 for precipitation to obtain a precipitated solid containing germanium, indium and tin; dissolving the precipitated solid containing germanium, indium and tin in a second acid solution to obtain a test solution; and testing the test solution by inductively coupled plasma mass spectrometry to obtain the element contents of germanium, indium and tin in the polymetallic ore sample. The present invention performs high-temperature melting decomposition of polymetallic ore with the assistance of sodium peroxide, which is conducive to the opening of the crystal structure of the polymetallic mineral, and facilitates the decomposition of the scattered elements germanium (Ge), indium (In) and tin (Sn) in the form of ions from the mineral structure. The present invention introduces ammonium hydroxide-ammonium salt buffer solution (NH3·H2O-NH4Cl) for leaching, and uses ferric hydroxide (Fe(OH)3) as a carrier to adsorb and precipitate the leached germanium ions, indium ions, and tin ions to achieve separation of matrix elements and large solvent sodium salts from target elements (germanium, indium, and tin), thereby effectively reducing matrix interference. The present invention dissolves and dilutes the precipitate with acid, and then determines it with inductively coupled plasma mass spectrometry (ICP-MS) to achieve accurate determination of germanium, indium, and tin elements at the same time. DETAILED DESCRIPTION

[0033] The present invention provides a method for simultaneously determining the contents of germanium, indium and tin in a polymetallic ore, comprising the following steps:

[0034] Mixing and melting the polymetallic ore sample and sodium peroxide to obtain a molten material;

[0035] The molten material, the ammonium hydroxide-ammonium salt buffer solution, and the ferric hydroxide are mixed for leaching, and then mixed with the first acid solution for acid dissolution to obtain a mixed solution;

[0036] The pH value of the mixed solution is adjusted to 9-10 for precipitation to obtain a precipitated solid containing germanium, indium and tin;

[0037] Dissolving the precipitated solid containing germanium, indium and tin in a second acid solution to obtain a test solution;

[0038] The test solution is tested by inductively coupled plasma mass spectrometry to obtain the element contents of germanium, indium and tin in the polymetallic ore sample.

[0039] The present invention mixes and melts a polymetallic ore sample and sodium peroxide to obtain a melt. In the present invention, the polymetallic ore sample preferably includes germanium-rich lead-zinc ore, copper ore, germanium ore, galena or zinc ore, and more preferably germanium-rich lead-zinc ore, germanium ore or zinc ore. In the present invention, the zinc ore is preferably sphalerite. In the present invention, the mass ratio of the polymetallic ore sample and sodium peroxide is preferably 0.1-0.2:2.0-3.0, and more preferably 0.1-0.2:2.5. In the present invention, the mixing is preferably carried out under stirring conditions, and the present invention has no special requirements for the stirring, as long as it can be mixed evenly. The present invention preferably mixes the polymetallic ore sample and part of the sodium peroxide, places the mixture in a corundum crucible, spreads the remaining part of the sodium peroxide on the surface of the mixture, and then places the mixture in a muffle furnace for melting; the purpose of spreading part of the sodium peroxide on the surface of the mixture of the polymetallic ore sample and sodium peroxide in the present invention is to promote the full decomposition of the polymetallic ore sample, and at the same time prevent the violent reaction during high-temperature melting, and splashing and loss.

[0040] In the present invention, the melting temperature is preferably 700-800° C., more preferably 750° C.; the melting time is preferably 10-20 min, more preferably 15-18 min.

[0041] In the present invention, after the melting, the process preferably further comprises: cooling the melted system to obtain a melt. In the present invention, the temperature after the cooling is preferably 20 to 50° C., more preferably 30 to 40° C. The present invention has no special requirements for the cooling method, as long as it can be cooled to the required temperature.

[0042] After obtaining the melt, the present invention mixes the melt, ammonium hydroxide-ammonium salt buffer solution, and iron hydroxide for leaching, and then mixes with the first acid solution for acid dissolution to obtain a mixed solution. In the present invention, the ammonium hydroxide-ammonium salt buffer solution is preferably an ammonium hydroxide-ammonium chloride buffer solution, and the pH value of the ammonium hydroxide-ammonium salt buffer solution is preferably 9.5-9.8, and more preferably 9.8. In the present invention, the temperature of the ammonium hydroxide-ammonium salt buffer solution is preferably 90-100°C, and more preferably 98-100°C; the mass of the polymetallic ore sample and the volume ratio of the ammonium hydroxide-ammonium salt buffer solution are preferably 0.1-0.2g:45-55mL, and more preferably 0.1-0.2g:50mL.

[0043] In the present invention, the mass ratio of the polymetallic ore sample to ferric hydroxide is preferably 0.1-0.2 g: 5.0-10.0 mg, more preferably 0.1-0.2 g: 5.0 mg. In the present invention, the mass concentration of ferric hydroxide in the mixed solution is preferably 0.1-0.2 g / L. In the present invention, the ferric hydroxide is a coprecipitation carrier that can capture and adsorb the target elements germanium, indium, and tin.

[0044] In the present invention, the leaching is preferably heated leaching, the leaching temperature is preferably 98-110° C., more preferably 100° C.; the leaching time is preferably 1.5-2.5 min, more preferably 2 min.

[0045] In the present invention, the leaching preferably further comprises: cooling the leached system and washing the corundum crucible with a nitric acid aqueous solution. In the present invention, the mass concentration of the nitric acid aqueous solution is preferably 45-55%, more preferably 50%.

[0046] After washing out the corundum crucible, the present invention preferably further comprises: washing the wall of the container containing the leaching solution. The present invention can make the elements to be tested remaining on the surface of the wall enter the leaching solution through water washing to ensure the accuracy of the detection data.

[0047] In the present invention, the first acid solution is preferably a nitric acid solution or a hydrochloric acid solution, more preferably a nitric acid solution; the mass concentration of the first acid solution is preferably 48-52%, more preferably 50%. The present invention utilizes the first acid solution to dissolve the iron hydroxide solid in the system after leaching. In the present invention, the pH value of the acid-soluble system is preferably below 7, more preferably 2-4, more preferably 2.5-3.0. The present invention has no special requirements for the amount of the first acid solution, as long as the pH value of the acid-soluble system can meet the above requirements. The present invention limits the pH value of the acid-soluble system to the above range, which is conducive to the complete dissolution of iron hydroxide.

[0048] After obtaining the mixed solution, the present invention adjusts the pH value of the mixed solution to 9-10 for precipitation to obtain a precipitated solid containing germanium, indium and tin. In the present invention, the pH value adjuster used to adjust the pH value of the mixed solution to 9-10 is preferably ammonia water; the mass concentration of the ammonia water is preferably 45-55%, more preferably 50%. The present invention has no special requirements for the amount of ammonia water, as long as the pH value of the system can reach the desired range. In the present invention, the main solid component in the precipitated solid containing germanium, indium and tin is ferric hydroxide, and germanium, indium and tin mainly exist in the form of ions.

[0049] In the present invention, after the precipitation, it is preferred that the method further comprises: subjecting the system after the precipitation to solid-liquid separation, and the solid-liquid separation is preferably filtration. In the present invention, the filtration is preferably performed by filtering with slow filter paper. In the filtration process of the present invention, it is preferred that the container containing the system after the precipitation is washed with water and then filtered. In the present invention, it is preferred that the solid obtained by the solid-liquid separation is washed with water 2 to 3 times to obtain a precipitated solid containing germanium, indium and tin.

[0050] After obtaining the precipitated solid containing germanium, indium and tin, the present invention dissolves the precipitated solid containing germanium, indium and tin in a second acid solution to obtain a test solution. In the present invention, the second acid solution is preferably a nitric acid solution; the mass concentration of the second acid solution is preferably 45-55%, more preferably 50%. The present invention has no special limitation on the amount of the second acid solution, as long as it can be completely dissolved.

[0051] In the present invention, after the dissolution, it is preferred that the following steps are further included: diluting and fixing the dissolved system to obtain the liquid to be tested. In the present invention, the dilution and fixing the volume can adapt the concentration of the liquid to be tested to the concentration required by the instrument. The present invention has no special limitation on the fixing reagent, and a conventional fixing reagent can be used. The present invention has no special limitation on the multiple of the dilution, and it can be adjusted according to the concentration of the solution. In the present invention, the filter paper for solid-liquid separation is preferably washed with water during the dissolution process, and the washed system is transferred to the dissolution system. The present invention can collect the acid solution remaining on the surface of the filter paper by washing the filter paper with water, thereby further improving the detection accuracy.

[0052] After obtaining the liquid to be tested, the present invention performs an inductively coupled plasma mass spectrometry test on the liquid to be tested to obtain the element contents of germanium, indium, and tin in the polymetallic ore sample. The present invention has no special limitation on the test method of the inductively coupled plasma mass spectrometry test, and a conventional method in the art can be used. In the present invention, the test conditions of the inductively coupled plasma mass spectrometry (ICP-MS) test preferably include:

[0053] The nebulizer was a high-sensitivity concentric nebulizer with a nebulization chamber temperature of 2.70°C;

[0054] RF power is 1550W;

[0055] The carrier gas is argon with a purity greater than 99.99%, and the carrier gas flow rate is 1.05L / min;

[0056] The auxiliary gas flow rate is 0.90L / min;

[0057] The helium flow rate is 5.0 mL / min;

[0058] The peristaltic pump speed is 40 rpm;

[0059] The sampling cone / interceptor cone are both nickel cones, the sampling cone diameter is 1.1mm, and the interceptor cone diameter is 0.5mm; the sampling mode is peak jumping; the sampling depth is 5.0mm; and the number of repetitions is 5 times.

[0060] In the present invention, the inductively coupled plasma mass spectrometry test is preferably an internal standard method; the internal standard solution used in the inductively coupled plasma mass spectrometry test process is preferably a rhodium (Rh) element standard solution and a rhenium (Re) element standard solution. In the present invention, the rhodium element standard solution is used to calibrate germanium, and the rhenium element standard solution is used to calibrate indium and tin. The present invention preferably mixes the test solution and the internal standard solution online before testing to achieve compensation correction and effectively reduce the matrix interference of the mass spectrometer. The present invention preferably injects the internal standard solution online through a three-way connection.

[0061] In the present invention, during the test of the sample to be tested by ICP-MS, the standard solution preparation method is preferably: using 2% nitric acid to dilute the standard solutions of germanium and tin step by step into a series of mixed standard solutions with concentrations of 0.00 μg / L, 0.50 μg / L, 1.00 μg / L, 5.00 μg / L, 10.0 μg / L, 50.0 μg / L, 100 μg / L, 500 μg / L, and 1000 μg / L. Using 2% nitric acid to dilute the standard solution of indium step by step into a series of mixed standard solutions with concentrations of 0.00 μg / L, 0.10 μg / L, 0.50 μg / L, 1.00 μg / L, 5.00 μg / L, and 10.0 μg / L. The present invention detects the standard solution and fits the test results to obtain a standard curve. The standard curve equation is as follows: Ge:f(x)=26963.0200x+16.396, R 2 =0.9998;In:f(x)=157125.3836x+118.7903,R 2 =0.9999;Sn:f(x)=39181.6659x+287.3654,R 2 =0.9997.

[0062] The present invention first melts the polymetallic ore sample by sodium peroxide-high temperature alkali fusion method, then extracts it in a system containing ammonium salt buffer solution and ferric hydroxide, and makes the target element coprecipitate by carrier coprecipitation adsorption means, and the germanium, indium and tin elements are adsorbed in the solid precipitate, and a large amount of matrix and solvent sodium salt are separated by solid-liquid separation, and the test liquid is purified; finally, the target element in the precipitate is dissolved by acid dissolution to obtain the test liquid, which can be directly measured on the machine, and the target element response value and concentration result are not affected by the dilution of the test solution, and are more suitable for the analysis and determination of actual samples. The determination method provided by the present invention is simple and fast to operate, and the results are accurate and reliable; the method detection limit, precision and accuracy are analyzed and verified by national standard substances, and the results meet the analysis and detection requirements of actual samples.

[0063] The testing method provided by the present invention is more suitable for the decomposition of polymetallic ore samples. High-temperature alkali fusion not only opens the mineral lattice, but also, under the precipitation adsorption of the precipitant (ferric hydroxide) and the use of ammonium salt buffer solution, by adjusting the pH value of the leaching solution, the target germanium, indium and tin elements can be effectively precipitated out. After filtration, most of the matrix elements and the solvent sodium salt are separated and removed, and the interference of the matrix and the sodium salt is reduced. It not only solves the problem that conventional acid dissolution or closed acid dissolution methods are difficult to digest the high content of silicon, aluminum, iron, titanium, zirconium, tin and other insoluble elements in actual samples, but also makes up for the problem that other measuring instruments such as atomic fluorescence spectrometry, flame atomic absorption spectrometry or AC arc-emission spectrometry cannot be used simultaneously with a set of pre-treatment system and on-machine measurement.

[0064] This method can accurately determine the content of germanium, indium and tin elements in polymetallic ores, and can provide basic technical support for the development and utilization of key strategic mineral resources.

[0065] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0066] The contents of some metal elements in the actual metal ore samples used in the examples are shown in Table 1. The metal element contents are determined according to the fourth edition of Rock and Mineral Analysis and the current national standard GB / T14353 series of methods.

[0067] Table 1 Actual polymetallic ore sample codes and partial metal element information used in the examples

[0068]

[0069] Example 1

[0070] The mineral samples collected from a polymetallic mining area in Guizhou were used as the samples to be tested, and were recorded as DF-1, DF-2, DF-3, DF-4, DF-5, DF-6, and DF-7;

[0071] 0.1 g (accurate to 0.0001 g) of the sample to be tested is placed in a corundum crucible, about 2.5 g of sodium peroxide is added, and after stirring and mixing, 0.5 g of sodium peroxide is spread on the surface of the mixture, and the mixture is placed in a muffle furnace and melted at 750°C for 15 minutes; cooled to 30°C to obtain a melt;

[0072] The melt is placed in a beaker containing 50 mL of an ammonium hydroxide-ammonium chloride buffer solution having a pH value of 9.8 and a temperature of 95° C., and about 5.0 mg of ferric hydroxide (Fe(OH)3) is added and heated to boil for 2 min for leaching, the leached system is cooled, the beaker wall is washed with water, and the corundum crucible is washed out with a 50% nitric acid aqueous solution; the leached system is further acidified with a 50% nitric acid aqueous solution to make its pH value 3.0, so that the ferric hydroxide is dissolved to obtain a mixed solution;

[0073] Using a 50% ammonia aqueous solution to adjust the pH value of the mixed solution to 9-10 for precipitation, filtering the system after precipitation with slow filter paper (washing the beaker and precipitating 2-3 times with water) to obtain a precipitated solid containing germanium, indium and tin;

[0074] Use 40mL of 50% nitric acid to dissolve the precipitated solid containing germanium, indium and tin in portions (wash the filter paper three times and transfer the washed system to the dissolution system), and place it in a 100mL volumetric flask. Dilute and fix the dissolved solution to obtain the test solution.

[0075] The liquid to be tested was tested by ICP-MS according to the internal standard method to obtain the element contents of germanium, indium and tin in the sample to be tested; a blank test was performed simultaneously (the preparation method of the blank sample was: the liquid to be tested was prepared according to the pretreatment method in Example 1, except that the sample to be tested was not added during the alkali fusion process);

[0076] Wherein, the standard solution is prepared by using 2% nitric acid to dilute the standard solutions of germanium, indium and tin step by step into a series of mixed standard solutions with concentrations of 0.00μg / L, 0.50μg / L, 1.00μg / L, 5.00μg / L, 10.0μg / L, 50.0μg / L, 100μg / L, 500μg / L and 1000μg / L. The standard solution of indium is diluted step by step into a series of mixed standard solutions with concentrations of 0.00μg / L, 0.10μg / L, 0.50μg / L, 1.00μg / L, 5.00μg / L and 10.0μg / L. The standard solution is tested and the test results are fitted to obtain a standard curve. The standard curve equation is: Ge:f(x)=26963.0200x+16.396, R 2 =0.9998;In:f(x)=157125.3836x+118.7903,R 2 =0.9999;Sn:f(x)=39181.6659x+287.3654,R 2 =0.9997.

[0077] Internal standard solution:

[0078] Rhodium and rhenium standard solutions with a mass concentration of 10 μg / L were used as internal standard solutions.

[0079] The test conditions of ICP-MS are:

[0080] The nebulizer was a high-sensitivity concentric nebulizer with a nebulization chamber temperature of 2.70°C;

[0081] RF power is 1550W;

[0082] The carrier gas is argon with a purity greater than 99.99%, and the carrier gas flow rate is 1.05L / min;

[0083] The auxiliary gas flow rate is 0.90L / min;

[0084] The helium flow rate is 5.0 mL / min;

[0085] The peristaltic pump speed is 40 rpm;

[0086] The sampling cone / interceptor cone are both nickel cones, the sampling cone diameter is 1.1mm, and the interceptor cone diameter is 0.5mm; the sampling mode is peak jumping; the sampling depth is 5.0mm; and the number of repetitions is 5 times.

[0087] The test results of Example 1 are listed in Tables 2 to 4. The contents of germanium, indium and tin in standard samples (GBW07729, GBW07832, GBW07237, GBW07163 and GBW07164) were tested according to the method of Example 1, and the results are listed in Tables 2 to 4.

[0088] The content of germanium in the test samples DF-1, DF-2, DF-3, DF-4, DF-5, DF-6, DF-7 and the standard sample was detected by atomic fluorescence spectrometry according to GB / T 14353.14-2014, and the results are listed in Table 2.

[0089] The content of indium in the test samples DF-1, DF-2, DF-3, DF-4, DF-5, DF-6, DF-7 and the standard sample was detected by referring to the mixed acid dissolution-ICP-MS test method in GB / T 14353.13-2014. The results are listed in Table 3.

[0090] The tin content in the test samples DF-1, DF-2, DF-3, DF-4 and the standard sample was detected by referring to the hydride generation atomic fluorescence spectrometry in GB / T 14353.19-2019 and the AC arc-emission spectrometry in DZ / T0279.11-2016. The results are listed in Table 4.

[0091] Table 2 Germanium content in ore samples

[0092]

[0093]

[0094] Table 3 Indium content in ore samples

[0095]

[0096] Table 4 Tin content in ore samples

[0097]

[0098]

[0099] It can be seen from Tables 2 to 4 that the detection method provided by the present invention can simultaneously detect the element contents of germanium, indium and tin in polymetallic ores. Compared with the reference method, the detection result of Example 1 of the present invention on the standard sample is basically within the uncertainty range of the standard value, indicating that the detection method provided by the present invention has a high detection accuracy.

[0100] In order to verify the reliability and accuracy of the method, the detection limit and lower limit of determination of the method were determined with reference to DZ / T 0451-2023: the blank experiment was repeated 7 times and the test results are listed in Table 5.

[0101] Table 5 Blank test results

[0102]

[0103]

[0104] The detection limit requirement of the method for germanium detected by referring to the method of GB / T 14353.14-2014 is 0.021 mg / kg; the detection limit requirement of the method for indium detected by referring to the method of GB / T 14353.13-2014 is 0.004 mg / kg; the detection limit requirement of the method for tin detected by referring to the method of DZ / T0279.11-2016 is 0.60 mg / kg. It can be seen from Table 5 that the detection method provided by the present invention has a lower detection limit and lower limit of determination, and the difference with the reference standard method is not significant.

[0105] Method detection precision and accuracy: The method of Example 1 of the present invention was used to detect standard samples GBW07832, GBW07237, GBW07164, GBW07165 and GBW07168 with different content levels for 7 times, and the test results are listed in Table 6.

[0106] Table 6 Test results of standard samples

[0107]

[0108]

[0109]

[0110] It can be seen from Table 6 that according to the detection method provided by the present invention, the relative standard deviations of germanium are 1.28%, 3.12%, 8.82%, 4.84%, and 3.83%, and the relative errors are -0.98%, 1.54%, 14.9%, 8.06%, and -5.15%; the relative standard deviations of indium are 1.70%, 17.9%, 7.70%, 1.64%, and 3.18%, and the relative errors are -5.48%, 13.2%, 2.92%, -3.59%, and 15.9%; the relative standard deviations of tin are 1.08%, 0.98%, and 0.87%, and the relative errors are 5.06%, 1.47%, and -6.43%; the parameters meet DZ / T 0130.3-2006 quality control requirements, indicating that the detection method provided by the present invention has high detection precision and accuracy, and the detection method provided by the present invention is feasible, reliable and accurate.

[0111] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for simultaneously determining the content of germanium, indium and tin in polymetallic ores. The following steps are involved: Mixing and melting the polymetallic ore sample and sodium peroxide to obtain a molten material; The molten material, the ammonium hydroxide-ammonium salt buffer solution, and the ferric hydroxide are mixed for leaching, and then mixed with the first acid solution for acid dissolution to obtain a mixed solution; The pH value of the mixed solution is adjusted to 9-10 for precipitation to obtain a precipitated solid containing germanium, indium and tin; Dissolving the precipitated solid containing germanium, indium and tin in a second acid solution to obtain a test solution; The test solution is tested by inductively coupled plasma mass spectrometry to obtain the element contents of germanium, indium and tin in the polymetallic ore sample.

2. The determination method according to claim 1, It is characterized in that The mass ratio of the polymetallic ore sample to sodium peroxide is 0.1-0.2:2.0-3.

0.

3. The determination method according to claim 1 or 2, It is characterized in that The melting temperature is 700-800° C. and the melting time is 10-20 minutes.

4. The determination method according to claim 1, It is characterized in that The pH value of the ammonium hydroxide-ammonium salt buffer solution is 9.5 to 9.8; The volume ratio of the mass of the polymetallic ore sample to the ammonium hydroxide-ammonium salt buffer solution is 0.1-0.2 g:45-55 mL; The mass ratio of the polymetallic ore sample to iron hydroxide is 0.1-0.2 g: 5.0-10.0 mg; The polymetallic ore samples include germanium-rich lead-zinc ore, copper ore, germanium ore, galena or zinc ore.

5. The determination method according to claim 1, It is characterized in that The extraction temperature is 98-110° C. and the extraction time is 1.5-2.5 min.

6. The determination method according to claim 1, It is characterized in that The first acid solution is a nitric acid solution or a hydrochloric acid solution; the mass concentration of the first acid solution is 48-52%.

7. The determination method according to claim 1, It is characterized in that The second acid solution is a nitric acid solution; the mass concentration of the second acid solution is 45-55%.

8. The determination method according to claim 1, It is characterized in that The pH value regulator used to adjust the pH value of the mixed solution to 9-10 is ammonia water; the mass concentration of the ammonia water is 45-55%.

9. The determination method according to claim 1, It is characterized in that The test conditions of the inductively coupled plasma mass spectrometry test include: The nebulizer was a high-sensitivity concentric nebulizer with a nebulization chamber temperature of 2.70°C; RF power is 1550W; The carrier gas is argon with a purity greater than 99.99%, and the carrier gas flow rate is 1.05L / min; The auxiliary gas flow rate is 0.90L / min; The helium flow rate is 5.0 mL / min; The peristaltic pump speed is 40 rpm; The sampling cone / interceptor cone are both nickel cones, the sampling cone diameter is 1.1mm, and the interceptor cone diameter is 0.5mm; the sampling mode is peak jumping; the sampling depth is 5.0mm; and the number of repetitions is 5 times.

10. The determination method according to claim 1 or 9, It is characterized in that The inductively coupled plasma mass spectrometry test is an internal standard method.

Citation Information

Cited By

  • Method for measuring content of noble metal elements in automobile purification catalyst

    CN121933502A